Home / notes / Materials Engineering Unit 5 Notes – Creep, NDT and Temperature-Dependent Behaviour

Materials Engineering Unit 5 Notes – Creep, NDT and Temperature-Dependent Behaviour

BME303 Unit 5 notes covering creep, fracture, fatigue, NDT methods, cryogenic and high-temperature behaviour, solved problems and answered PYQs.

Course Code: BME303

Course: AKTU B.Tech 2nd Year, Semester III

Unit: Creep, NDT and Temperature-Dependent Behaviour

Stream: Mechanical Engineering (ME)

Unit V Overview

Understand time-dependent deformation and failure; compare every NDT method in the supplied syllabus; and explain how low and high temperatures change properties. Read labelled apparatus and signal diagrams, practise calculations and justify inspection choices.

Topics Covered

Syllabus area Pages
Creep curves, mechanisms and models 2-7
Fracture, fatigue and failure analysis 7-9
NDT foundations, VT, PT and MT 9-12
Ultrasonic and acoustic methods 12-15
Radiography, XRD and eddy currents 15-19
Method selection and evaluation 19-20
Cryogenic behaviour and contraction 21-23
High-temperature behaviour and review 23-26
Worked problems 26-28
Quick revision checks 28-28
Formula quick reference 29-29
PYQs with Answers 30-43

Learning Outcomes

  • 1. Read creep curves and explain failure.

  • 2. Choose NDT by material and flaw type.

  • 3. Interpret echoes, images and diffraction.

  • 4. Calculate rates, depths and thermal movement.

  • 5. Compare cryogenic and hot-service behaviour.

Included in These Notes

50 explained sections; 44 core diagrams and charts; 10 realistic illustrative images; 10 solved problems; comparison tables; 6 concise revision checks; a formula sheet; and 21 PYQs with answers.

Study Approach

Visualise. Follow the physical mechanism, apparatus and signal path.

Calculate. State the units, geometry and supplied model.

Interpret. Link the observation to a justified engineering conclusion.

Key checks: Use kelvin for temperature ratios; UT echo time is a round trip; XRD uses θ, not 2θ; a test indication is not automatically a defect.

1. Creep: deformation that depends on time

Creep is progressive, time-dependent deformation under a sustained mechanical load or stress. A component can therefore distort even though its initial stress is below the short-term tensile yield strength. Turbine parts, steam pipes and furnace supports must be assessed for their operating time as well as their initial strength.

The total measured strain contains the instantaneous loading strain and the subsequent time-dependent contribution. Write εtotal = εinitial + εcreep when separating these parts. Creep strain is not automatically recovered on unloading; elastic recovery must not be confused with the permanent deformation already accumulated.

Figure 5.1
Typical total strain under sustained loading; the vertical start represents instantaneous loading strain.

Temperature, stress, microstructure, environment and time all affect the response. Metals commonly show engineering-significant creep at elevated homologous temperature; polymers may creep near room temperature. A single universal temperature boundary cannot describe every material.

Visual 5.1
A controlled creep machine records extension while maintaining the selected load and specimen temperature. Illustrative view.

2. Reading the three stages of a creep curve

A constant-load creep test commonly produces three recognisable regions. In primary creep, the strain rate decreases as deformation resistance develops. In secondary creep, competing hardening and recovery processes can produce an approximately steady minimum rate. In tertiary creep, damage and section reduction accelerate deformation towards rupture.

The secondary region is a useful design descriptor, but a perfectly straight segment is an idealisation. Some materials or test conditions do not display three sharply separated stages. The end of a plotted test may also represent termination rather than actual rupture; read the accompanying test record.

Figure 5.2
Primary rate decreases, secondary rate is approximately steady, and tertiary damage accelerates deformation.

The slope of a strain-time curve is creep rate. A small strain at a short inspection interval does not establish a safe long-term life. Compare the operating stress, temperature and exposure with relevant creep and rupture data rather than extrapolating the initial elastic response.

3. Creep rate and the strain budget

An average creep rate over an interval is Δε/Δt. If strain is dimensionless and time is in seconds, the rate has units s^(-1). A rate quoted in percent per hour requires both the percentage conversion and the hour-to-second conversion before substitution into an SI equation.

For an approximately constant secondary rate, the additional strain is rate multiplied by time. Add any supplied initial and primary strain when a problem asks for total extension. For a gauge length L0, extension is approximately L0 ε when the stated strain measure is engineering strain.

Figure 5.3
The slope of the strain-time curve is creep rate. The near-minimum region is not a prediction of rupture time.

Use the steady-rate approximation only over the interval for which it is supplied. It does not describe accelerating tertiary deformation. A component may exceed an allowable distortion before rupture, so a strain limit and a rupture-life limit are different design conditions.

4. Homologous temperature: always use kelvin

Homologous temperature is TH = T/Tm, where both the operating temperature and melting temperature are absolute temperatures. Convert degrees Celsius by adding 273.15. A ratio made directly from Celsius values has no physical meaning because the Celsius zero is arbitrary.

Diffusion and recovery become increasingly important as homologous temperature rises. A rule of thumb near 0.4 Tm is often useful for discussing creep in metals, but it is not a universal design threshold. Stress level, alloy chemistry, grain size and service duration can make appreciable creep occur outside a simple rule.

Figure 5.4
Illustrative absolute-temperature ratios; the dashed reference is a guide, not a universal allowable limit.

Materials with very different melting temperatures can experience very different creep severity at the same Celsius temperature. For alloys, melting may occur over a range; the reference temperature must be stated. In examinations, use the melting temperature supplied by the question.

5. How a creep test is performed

A creep test applies a specified tensile load or stress while maintaining a controlled specimen temperature. The gauge extension is recorded with time, often using extensometry arranged to minimise errors from the hot zone. Temperature uniformity, alignment and an accurate initial gauge length are essential to meaningful results.

In a constant-load test, the engineering stress based on the original area remains constant. The true stress can rise as the specimen thins. A constant-true-stress test requires load adjustment and is not the same experiment. Always identify the control condition when comparing curves.

Figure 5.5
A controlled furnace surrounds the loaded gauge section while extension and temperature are measured.

A creep-rupture test records time to fracture under specified conditions, while a creep test may stop at a selected time or strain. The data record should state material condition, specimen dimensions, temperature history, load, strain measurement and whether rupture occurred.

6. Dislocation creep and recovery

At elevated temperature, dislocations can move by glide and can climb when diffusion permits motion out of their original slip plane. Climb helps dislocations bypass obstacles. The resulting deformation depends on both the applied stress and the thermally activated processes available in the microstructure.

During secondary creep, deformation tends to increase dislocation density while recovery rearranges or removes dislocations. An approximate balance can produce a near-steady rate. This description explains a trend; it does not establish a numerical rate without material-specific data.

Figure 5.6
Glide and diffusion-assisted climb provide different routes for dislocation movement; lattice geometry is idealised.

Alloying, precipitates and stable dispersions can impede dislocation motion. Their benefit depends on stability during service: precipitate coarsening or dissolution may reduce long-term resistance. A steel that is strong in a rapid room-temperature test is not automatically resistant to years of high-temperature loading.

7. Diffusion creep and the role of grain size

Diffusion creep involves stress-directed movement of atoms and vacancies. Nabarro-Herring creep is associated with diffusion through the lattice; Coble creep involves grain-boundary diffusion. These mechanisms are most relevant in suitable combinations of temperature, stress and grain size rather than under every service condition.

In simple idealised models, the lattice-diffusion contribution varies inversely with grain size squared, while the grain-boundary contribution varies inversely with grain size cubed. These dependencies explain why fine grains can accelerate diffusion creep. Apply such powers only when the question explicitly assigns the relevant mechanism and other factors are unchanged.

Figure 5.7
Lattice and grain-boundary pathways distinguish two ideal diffusion-creep mechanisms.

Fine grains can improve room-temperature yield strength yet be disadvantageous for some high-temperature creep conditions. This is a useful example of competing design objectives. Grain-boundary sliding can accompany deformation and contribute to damage if accommodation is inadequate.

8. Cavitation, section loss and tertiary damage

Creep cavities can nucleate at grain boundaries or particles, enlarge and link into cracks. At the same time, local necking reduces the load-bearing section. Under constant load, section reduction increases true stress and can accelerate the deformation rate further.

Tertiary creep is therefore associated with evolving damage as well as changes in specimen geometry. Oxidation or corrosion can remove additional section and weaken boundaries in some environments. A simple constant-rate estimate cannot represent all these effects.

Figure 5.8
Cavities can grow and link along a boundary under tensile loading; size and spacing are exaggerated.

Inspection may seek surface cracks, wall loss, distortion or microstructural evidence, using methods appropriate to the component. Absence of a visible crack does not establish absence of creep damage. Remaining-life assessment requires a combination of operating history, material condition and suitable validated measurements.

9. Stress dependence: a supplied Norton model

A common secondary-creep relation is creep rate = A σ^n at fixed temperature. The stress exponent n is fitted over a stated range; A carries the units needed for the chosen stress and time units. A and n are not universal constants for all creep mechanisms.

For the same material condition and temperature, a ratio calculation eliminates A: rate2/rate1 = (σ2/σ1)^n. This makes the effect of stress changes clear without inventing an absolute rate. Even a moderate stress increase can strongly increase the predicted rate when n is large.

Figure 5.9
Two supplied stress exponents illustrate different rate sensitivity; the curves are not fitted alloy data.

Do not extend a fitted power law through a change of mechanism or beyond its calibrated range. If stress is entered in MPa when A was defined for Pa, the answer can be wrong by many orders of magnitude. State the units beside the supplied relation.

10. Temperature dependence and creep-resistant design

A thermally activated model may be written creep rate = A σ^n exp[-Q/(RT)]. Q is activation energy per mole and R is the molar gas constant in consistent energy units. At unchanged stress, the rate ratio is exp[(Q/R)(1/T1 – 1/T2)]. Temperatures must be in kelvin.

The model shows why a small temperature increase can have a large long-term effect. Actual service predictions need an alloy-specific relation and a valid stress-temperature range. A fitted activation energy is an effective parameter and does not by itself prove a unique microscopic mechanism.

Figure 5.10
A supplied activation-energy model predicts increasing creep rate with absolute temperature at fixed stress.

Creep resistance can be improved through temperature control, reduced stress, stable strengthening phases and appropriate grain structure. Single-crystal turbine alloys remove grain boundaries but still creep. Environmental resistance and cooling design remain important alongside mechanical strength.

11. Rupture data and the limits of life estimates

A stress-rupture curve relates applied stress to rupture time at a specified temperature and material condition. A creep-strength value normally also refers to a stated time and allowable strain. Quoting a strength without its temperature and duration omits essential information.

A supplied time-temperature parameter, such as P = T(C + log10 tr), can combine test data for an engineering estimate. The constant C, temperature units, rupture-time units and applicable material condition must all be specified. A correlation is not a guarantee that every heat, weld or component follows the same curve.

Figure 5.11
Schematic stress-rupture trends: stress, temperature and time must be specified together.

Do not infer remaining life simply by subtracting elapsed time from a laboratory rupture time obtained at different conditions. Changes in load, temperature, section, environment or microstructure can alter damage development. In these notes, life calculations use explicitly supplied teaching models.

12. Failure analysis: collect evidence before deciding

Failure means inability to perform the intended function. It can involve fracture, excessive deformation, wear, leakage or loss of required properties. A broken part is the final observation; the engineering task is to identify the mechanism and the conditions that produced it.

Record the component location, loading direction, environment, temperature, service history and visible damage before cleaning or cutting. Preserve matching fracture halves where possible. Dimensional checks, material identification, metallography and suitable NDT can then test competing explanations.

Figure 5.12
Preserve evidence, examine condition, test possible mechanisms and then justify corrective action.

Separate the initiation site, the propagation mechanism and the final overload region. A fatigue crack can grow slowly and then finish by ductile overload. The final rough region alone must not be used to label the entire event. Corrective action should address the cause supported by the evidence.

13. Ductile and brittle fracture

Ductile fracture involves substantial local plastic deformation and often microvoid nucleation, growth and coalescence. A tensile specimen may show necking and a cup-and-cone appearance. The amount of deformation depends on the material, stress state, temperature and loading rate.

Brittle fracture involves limited macroscopic plastic deformation and may proceed by cleavage or along weakened grain boundaries. A flat-looking fracture is a clue, not a complete diagnosis. Notches, constraint and low temperature can make a normally ductile material behave less tolerantly.

Figure 5.13
Local necking contrasts with a low-plasticity fracture geometry; actual diagnosis needs more than appearance.

Fracture toughness describes resistance to crack extension under specified conditions and is different from tensile strength or impact energy. A high-strength material can have limited crack tolerance. The illustration shows typical features for comparison and does not replace microscopic examination of an actual failure.

Visual 5.2
Necked tensile-specimen halves illustrate ductile deformation before separation. Illustrative view.

14. Fatigue: repeated loading and crack growth

Fatigue is progressive damage under repeated or fluctuating loading. Cracks often initiate at surface defects, notches, inclusions or other stress concentrators. Propagation can occur even when the nominal maximum stress is below the monotonic yield strength.

For a simple cycle, stress amplitude σa = (σmax – σmin)/2 and mean stress σm = (σmax + σmin)/2. The stress ratio is R = σmin/σmax when σmax is nonzero. State whether the plotted quantity is amplitude, range or maximum stress.

Figure 5.14
Example cycle with a 50 MPa mean and 80 MPa amplitude. Stress range is twice the amplitude.

An S-N curve relates a specified stress measure to cycles to a defined failure criterion. Some steels show an endurance-limit behaviour under particular test conditions; many alloys do not have a true horizontal long-life limit. Surface condition, mean stress and environment affect the result, so a generic curve cannot establish a component life.

15. Creep, fatigue and environmental interaction

A hot component may experience sustained loads, thermal cycles and a reactive environment together. Creep-fatigue interaction can produce behaviour that is not predicted by treating each process independently. Hold times at high stress may be especially important to the damage mechanism.

Thermal fatigue arises when restrained or nonuniform temperature changes generate cyclic thermal stresses. Oxidation can assist surface crack initiation, while corrosion or hydrogen-related mechanisms may alter fracture behaviour in other service environments. Identify the actual material-environment combination rather than applying every mechanism to every alloy.

Figure 5.15
A schematic S-N trend; a horizontal endurance limit is not implied for every alloy.

A failure-analysis answer should connect service conditions to observed evidence and suitable verification. Recommend changes such as reducing thermal gradients, improving surface finish or altering material selection only when they address the proposed mechanism. A generic instruction to use a stronger material is rarely sufficient.

16. NDT: what an inspection result really means

Non-destructive testing examines material or component condition without intentionally impairing its intended use. Methods respond to different physical properties: optical visibility, capillary penetration, magnetic flux leakage, elastic waves, radiation attenuation, diffraction or electromagnetic induction.

An indication is an instrument or visual response. A discontinuity is an interruption in material structure. A defect is a discontinuity that fails the applicable acceptance requirements. These terms are related but not interchangeable: a visible indication is not automatically a rejectable defect.

Figure 5.16
Choose the physical method, interpret its response and evaluate it against the applicable requirements.

Inspection capability depends on flaw size, orientation, depth, access, surface condition, equipment, procedure and operator performance. No method proves that a component is completely flaw-free. Use a suitable combination of methods and report both the examined region and the limits of the examination.

17. Visual inspection: direct and remote access

Visual testing is often the first inspection stage. It can reveal accessible cracks, corrosion, distortion, poor weld profile, misalignment and surface damage. Direct inspection uses unaided or aided vision; remote inspection may use a borescope, camera or other optical arrangement.

Adequate lighting, viewing angle, cleanliness and a suitable scale are essential. A crack hidden by paint or an inaccessible internal surface may escape detection. A photograph without a size reference can record an appearance but may not support accurate dimensional evaluation.

Figure 5.17
Surface examination requires suitable illumination and a clear viewing path; internal depth is not established.

Use gauges or other measurements when an acceptance criterion specifies dimensions. Record the location and direction of an observed feature so that another examiner can find it again. Visual testing can guide the choice of a complementary method, but it does not independently establish the depth of a surface crack.

Visual 5.3
Lighting, magnification and accessible surfaces support visual weld inspection. Illustrative view.

18. Penetrant testing: the capillary principle

Liquid penetrant testing detects discontinuities that are open to the surface of a suitable nonporous material. A wetting liquid enters accessible openings; after excess surface penetrant is removed, a developer helps draw retained penetrant out to form a visible indication.

The method can be used on many metals and compatible nonmetallic materials. It does not reveal a sealed internal pore that has no surface connection. Porous surfaces can retain penetrant over a broad area and generate an unhelpful background rather than a clear crack indication.

Figure 5.18
Penetrant retained in a surface-connected opening produces a developed indication; the section is enlarged.

Visible-dye and fluorescent systems require their specified viewing conditions. Material compatibility, surface preparation and the approved penetrant-removal method matter. Penetrant colour on the surface is an indication of retained liquid; it is not a direct measurement of the true crack depth.

19. Penetrant process: from preparation to interpretation

Start with cleaning and drying so that openings are accessible. Apply penetrant and allow the specified dwell. Remove the excess using the selected system without washing penetrant out of discontinuities. Apply the appropriate developer, allow the specified development interval and examine under the required lighting.

After recording and evaluating relevant indications, clean the component as required for its next operation. The exact dwell, temperature range and cleaning chemistry depend on the approved procedure and product system. A single arbitrary timing recipe is not suitable for every material or surface condition.

Figure 5.19
Clean, penetrate, remove excess and develop. Dwell and viewing conditions come from the selected procedure.

Overcleaning can remove penetrant from shallow cracks; undercleaning can leave excessive background. Broad stains at corners or rough surfaces may be nonrelevant indications. Confirm their origin before evaluation. An examination record should distinguish a linear indication from an interpretation that it represents a crack.

Visual 5.4
A fine red indication develops against a contrasting developer layer; its origin still requires evaluation. Illustrative view.

20. Magnetic-particle testing: flux leakage

Magnetic-particle testing is used on ferromagnetic materials. A magnetic field is established in the component; a suitably oriented discontinuity can disturb the flux and create leakage near the surface. Fine magnetic particles accumulate at the leakage field and form an indication.

The method can detect surface and some near-surface discontinuities, depending on the magnetisation conditions and the discontinuity. It is not a general method for aluminium, copper or all stainless steels. Austenitic stainless steel is usually unsuitable because it is not ferromagnetic in its usual condition.

Figure 5.20
A crack crossing magnetic flux creates a local leakage field that attracts particles.

A yoke is one way to magnetise a local region. Adequate contact and field coverage are required. Particle application, surface contrast or fluorescent viewing, background and field direction influence sensitivity. The particle pattern must be evaluated under an applicable procedure rather than treated as an exact image of subsurface crack dimensions.

21. Magnetic field direction and examination coverage

A crack is generally most readily detected when it cuts across the magnetic field. If the field runs parallel to a narrow planar discontinuity, the disturbance may be much weaker. Two substantially different field directions help reduce this orientation limitation.

Coverage must include the required component area with adequate magnetisation. Changing the yoke position or using another magnetisation technique may be necessary around complex geometry. Edges, changes in section and permeability changes can produce nonrelevant indications that require interpretation.

Figure 5.21
A field across a crack generally gives a stronger response than a field parallel to it.

The procedure may require verification of field adequacy and demagnetisation after examination. Residual magnetism can attract particles or affect later operations. Magnetic testing is a local response to flux leakage; it cannot be assumed to detect every deeply buried flaw or supply a complete volumetric map.

Visual 5.5
An electromagnetic yoke establishes a local field in a ferromagnetic component. Illustrative view.

22. Ultrasonic testing: pulse, reflection and return

Conventional ultrasonic testing introduces high-frequency elastic waves through a transducer. At an interface with a change in acoustic impedance, part of the wave can be reflected. Pulse-echo equipment measures the returning signals and their arrival times.

A contact probe normally uses a couplant to bridge the air gap between probe and component. The wave mode and sound velocity depend on the material and arrangement. Longitudinal and shear waves have different velocities, so an incorrect velocity setting produces an incorrect distance estimate.

Figure 5.22
A contact probe sends and receives elastic waves; the echo includes the outward and return paths.

Reflection depends strongly on flaw orientation, size, surface and the sound beam. A planar crack parallel to the beam may give a weak response. Calibration on suitable reference features and a planned scanning pattern are therefore essential. Special methods such as EMAT or laser ultrasonics do not follow every conventional contact-couplant assumption.

Visual 5.6
A contact probe, couplant and flaw detector form a conventional pulse-echo examination arrangement. Illustrative view.

23. A-scan echoes and the factor of two

An A-scan plots signal amplitude against time or a calibrated distance axis. An entry response, a reflector echo and a back-wall echo may appear at different positions. The display is a signal record, not a photograph of the component interior.

For a normal-beam pulse-echo measurement after instrument delay correction, reflector depth d = ct/2. The measured time includes travel from probe to reflector and back. If a question already gives a one-way time, do not divide by two again.

Figure 5.23
Synthetic echoes illustrate time separation. Example reflector and back-wall times are 8 and 20 µs.

A back-wall echo can help check thickness when velocity and coupling are appropriate. A missing back-wall echo can have several causes, including poor coupling, attenuation, geometry or an intervening reflector. Treat it as evidence to investigate rather than automatic proof of a crack. Echo height alone is not a universal flaw-size measurement.

24. Angle-beam UT: sound path is not normal depth

An angle-beam probe directs a refracted beam into the component, often to examine welds. The angle used for simple geometry is the refracted beam angle in the material, not automatically the wedge angle. Clearly state whether the angle is measured from the surface or its normal.

If θ is measured from the surface normal, the one-way sound path s gives depth z = s cos θ and horizontal offset x = s sin θ. For a pulse-echo time, calculate s = ct/2 first. These expressions describe a straight first-leg path before reflection at the back wall.

Figure 5.24
First-leg geometry: the refracted angle is measured from the normal; sound path differs from depth.

Skip paths, curved surfaces and changing wave modes need additional geometry. Calibration and reference position remain necessary. A numerical answer based only on ct/2 gives the sound path; calling it the normal depth in an angle-beam question is a common error.

25. UT frequency, wavelength and practical limitations

Wavelength is λ = c/f. For the same wave mode and velocity, increasing frequency reduces wavelength and can improve the ability to resolve small features under suitable conditions. It can also increase attenuation and scattering in many engineering materials.

Coarse grains, complex geometry, surface roughness, the near-surface dead zone and unfavourable reflector orientation can limit examination. High frequency is therefore not automatically the best choice for a thick coarse-grained casting. Probe design, pulse length and focusing also affect resolution.

Figure 5.25
At unchanged wave speed, higher frequency gives shorter wavelength; attenuation must also be considered.

Use a reference block and a procedure suitable for the material and geometry. Record the examined volume, scanning direction, probe conditions and relevant indications. A claimed detection limit requires evidence from the actual inspection system, not merely a wavelength calculation.

26. Acoustic testing: resonance and vibration

Acoustic testing is a broad term. Tap or resonance methods observe how a component responds to mechanical excitation; changes in stiffness, mass, support or damage can alter the sound or vibration response. Such methods are useful for comparison when test conditions are controlled.

A ringing sound is not proof of complete structural integrity. Geometry, boundary conditions and contact can change the response even when the material is sound. Conversely, a small defect may not produce an easily recognised audible change.

Figure 5.26
Synthetic resonance curves show a possible response change; support and geometry can also shift a peak.

Instrumented resonance and vibration measurements can support screening or condition monitoring. Define the reference condition and the measured feature, such as resonance frequency or damping. This active excitation approach must be distinguished from acoustic emission, which listens for energy released by active sources within the loaded material.

27. Acoustic emission: listening to active damage

Acoustic emission detects transient elastic waves released by sources within a material, such as crack advance or certain deformation events. Sensors listen while the component is loaded or otherwise undergoing an active process. The system does not normally send a UT pulse into the part.

Several sensors can help locate an event by comparing arrival times. Wave speed, geometry, attenuation, reflections, threshold and sensor coupling affect the result. Friction, electrical noise and other non-damage sources can also generate signals that need to be separated from relevant activity.

Figure 5.27
Sensors listen for elastic waves released by active sources; they are not transmitting a UT interrogation pulse.

A dormant crack may emit little or no acoustic energy during an observation interval. Therefore, silence does not prove absence of a discontinuity. AE is valuable for monitoring active behaviour over an area; complementary local inspection is often needed to characterise a reported source.

28. Arrival-time localisation and UT versus AE

For a simple one-dimensional bar, place a left sensor at x = 0 and a right sensor at x = L. If an event occurs at x, the direct travel times are x/c and (L – x)/c. Defining Δt = tright – t_left gives x = (L – cΔt)/2.

The sign matters: an event nearer the left sensor reaches it first and produces a positive Δt under this definition. The formula assumes a known constant wave speed and direct arrival along the bar. Real plates and vessels can require wave-mode identification and more elaborate location procedures.

Figure 5.28
Direct arrivals at two sensors locate a source on an ideal straight bar when wave speed is known.

UT actively transmits a known pulse and studies its response. AE passively monitors generated events while the structure is active. Neither method replaces the other in every application. The choice depends on whether the task is local reflector examination or monitoring sources that are releasing energy.

Feature UT AE
Energy source Instrument pulse Active event in part
Main record Echo versus travel time Event timing and activity
Silent flaw May still reflect a pulse May produce no event

29. Radiography: source, component and detector

Radiographic testing forms a transmission image using penetrating radiation. An X-ray tube generates X-rays electrically; gamma radiography uses a suitable radionuclide source. Radiation passes through the component and reaches a film or digital detector.

Changes in thickness, density and composition affect transmitted intensity. Voids or missing material can increase transmission along a path. The displayed brightness depends on the recording and display convention: a more exposed region is often darker on conventional negative film, but digital polarity can be reversed.

Figure 5.29
Source-component-detector geometry forms an attenuation projection; a void changes the traversed material path.

Radiography provides a projection through the thickness. Superimposed features can make depth interpretation difficult, and some tight planar cracks are poorly detected when their orientation gives little path-length contrast. Shielding, controlled access and qualified operation are part of the examination arrangement, not optional additions.

Visual 5.7
An inactive shielded inspection cabinet shows the component position between the source and detector. Illustrative view.

30. Attenuation and radiographic contrast

An ideal narrow monoenergetic beam obeys I = I0 exp(-μx), where μ is the linear attenuation coefficient and x is path length. If μ is in mm^(-1), x must be in millimetres. The ratio I/I0 is dimensionless.

A thicker path or a larger attenuation coefficient gives lower transmitted intensity. A void reduces the absorbing path, which can change detector exposure. Real industrial X-ray beams are often polychromatic; scattering, beam hardening, detector response and image processing complicate the simple model.

Figure 5.30
The ideal monoenergetic attenuation model predicts continuously decreasing transmission with thickness.

Radiographic contrast and spatial resolution are separate concepts. A high intensity difference is useful only if the image also resolves the required feature. Use supplied coefficients and geometry for teaching calculations, and do not infer an exposure procedure or guaranteed detection threshold from the ideal attenuation equation alone.

31. Radiographic geometry and image quality

A finite source size produces geometric unsharpness. In a simple arrangement, Ug = F b/a, where F is effective source size, a is source-to-object distance and b is object-to-detector distance. Reducing the detector gap or increasing source distance reduces this geometric contribution.

Image quality also depends on motion, scatter, detector characteristics and the selected examination technique. An image-quality indicator helps demonstrate a specified aspect of the radiographic technique; it does not prove that every real defect will be detected.

Figure 5.31
Finite source size spreads the projected edge; reducing detector gap decreases geometric unsharpness.

Keep the source-object-detector geometry clear in a labelled sketch. A component image may contain overlapping walls or structural features. Interpret an indication with the component drawing and exposure arrangement, and use complementary views or another method when location or orientation remains uncertain.

32. X-ray diffraction is different from radiography

X-ray diffraction studies constructive interference from regularly spaced atomic planes. It is useful for crystal-structure and phase analysis, lattice-spacing measurement, texture studies and appropriate residual-stress measurements. Radiography instead forms an attenuation projection through a component.

For a given set of planes, Bragg diffraction satisfies nλ = 2d sin θ. The angle θ is the angle between the incident beam and the lattice planes in the simple reflection construction. A conventional powder pattern is commonly plotted against 2θ, so the plotted peak angle must be halved before using Bragg law.

Figure 5.32
Bragg geometry distinguishes θ from the scattering angle 2θ. The dotted ray continues the incident direction.

A diffraction peak is not a picture of a pore or crack. Phase identification normally uses several peak positions and intensities with suitable reference data. Instrument geometry, specimen preparation and texture can affect the observed pattern.

Visual 5.8
An enclosed diffractometer measures diffraction from a prepared specimen. Illustrative view.

33. Reading a diffraction pattern and lattice strain

Peak positions encode lattice spacing through Bragg law. Peak intensities depend on structure and measurement conditions; their variation is not simply the amount of a phase without an appropriate analysis. Peak broadening can contain information about crystallite size, strain and instrument effects, which must be separated.

A simple lattice strain along the measured direction is ε = (d – d0)/d0. Here d0 is an appropriate stress-free reference spacing. Converting that strain into residual stress needs suitable elastic constants, geometry and assumptions; it is not always the uniaxial formula Eε.

Figure 5.33
Synthetic peak positions illustrate a 2θ pattern; no measured phase identification is claimed.

A shift towards lower 2θ at fixed wavelength corresponds to larger d for the same indexed reflection. Do not compare peaks from different planes as if they were a strain pair. Conventional laboratory reflection measurements usually probe a limited near-surface region rather than the entire component thickness.

34. Eddy-current testing: electromagnetic induction

An alternating current in a probe coil produces a changing magnetic field. When a conducting component is nearby, currents are induced in it. Their electromagnetic response changes the probe impedance, and discontinuities or material-property changes can alter the measured signal.

Electrical conductivity is essential; ferromagnetism is not required. Aluminium and copper can be examined, while an ordinary nonconducting ceramic cannot be tested by the same conventional induction mechanism. Ferromagnetic materials introduce permeability effects that can complicate interpretation.

Figure 5.34
An AC probe induces currents in a conducting part; a crack can disturb their paths and probe response.

Eddy-current testing is useful for surface and near-surface examination, tubing, fastener regions and some sorting or coating measurements. It usually needs no liquid couplant. Probe lift-off, edge effects, conductivity and permeability changes can mimic or obscure a flaw response, so calibration on an appropriate reference is essential.

Visual 5.9
A connected pencil probe examines a conducting panel near a fastener region. Illustrative view.

35. Skin depth, frequency and lift-off

For a simple homogeneous conducting half-space, skin depth δ = 1/√(π f μ σ), using SI units. Here f is frequency, μ is magnetic permeability and σ is electrical conductivity. Skin depth is the depth at which current amplitude falls to 1/e of its surface value in the ideal model.

At unchanged conductivity and permeability, increasing frequency by a factor of four halves skin depth. This does not establish a sharp inspection boundary: current decays continuously. Actual sensitivity also depends on coil geometry, material, flaw orientation and signal-to-noise ratio.

Figure 5.35
Ideal current amplitude falls to 1/e at one skin depth and continues decreasing below it.

Lift-off is separation between probe and conducting surface. Paint thickness or probe wobble can change it. A probe signal must therefore be interpreted against reference responses and controlled scanning conditions. Skin depth alone cannot supply an exact crack depth or a universal guaranteed penetration distance.

36. Choosing a complementary inspection combination

Start with the inspection objective: surface crack detection, internal volumetric examination, wall-thickness measurement, phase analysis or active-damage monitoring. Then identify the material, likely flaw geometry, access, surface condition and service constraints.

A nonporous aluminium part with a surface-breaking crack may suit penetrant or eddy-current examination, while magnetic-particle testing is inappropriate. A steel weld may need visual testing plus surface and volumetric methods chosen for its expected discontinuities. XRD can answer a phase question but is not a substitute for a crack-detection plan.

No simple ranking makes one method best for all defects. UT and radiography can complement each other because their responses to orientation and volume differ. State what each selected method contributes and what remains uncertain rather than listing many techniques without a purpose.

37. Calibration, recording and acceptance decisions

Calibration establishes the relationship between an instrument response and suitable known references. Reference blocks, known reflectors, dimensional standards or system checks must be appropriate to the method. Calibration does not remove all limitations associated with geometry or flaw orientation.

A useful report identifies the component, examined area, method, procedure, equipment settings, reference checks, surface condition and relevant indications. Locations should be reproducible using a drawing, coordinate or reference feature. Distinguish raw observations from interpretation and final evaluation.

Acceptance depends on the governing specification or engineering assessment. An indication amplitude or length is not a universal rejection criterion. When an examination is inconclusive, the appropriate response can be an additional view, another method or a qualified assessment rather than an unsupported declaration that the part is safe or defective.

NDT METHOD SELECTION MAP

Figure 5.36
Physical information and limitations of the listed NDT methods. This selection map summarises principles; component acceptance depends on the applicable examination requirements.
Decision What to establish
1 Material Ferromagnetism for MT; conductivity for ET; suitable nonporosity for PT.
2 Discontinuity Surface opening, internal volume, planar orientation, phase condition or active damage.
3 Access and geometry Surface preparation, coupling, beam direction, detector position and examination coverage.
4 Evaluation Calibrate, locate and interpret the response, then apply the governing acceptance requirements.

Remember: an indication is an observed response. A discontinuity becomes a defect only when it fails the applicable requirements. Complementary methods address different limitations.

38. Cryogenic service: temperature changes the problem

Cryogenic service refers to very low temperatures; a boundary near 120 K is often used in engineering discussion, but the application must state its operating range. Liquid-nitrogen and liquid-helium temperatures are very different conditions and should not be treated as interchangeable.

Low temperature can increase the strength of many metals while reducing ductility or fracture resistance in susceptible materials. Thermal contraction, joining, sealing and differential expansion become important even when the mechanical load is modest. Properties must be taken for the actual grade and material condition at the relevant temperature.

Figure 5.37
A temperature-controlled chamber conditions the gauge section for low-temperature mechanical testing.

A material selected only from a room-temperature tensile-strength table may be unsuitable. Evaluate toughness, fatigue behaviour, thermal conductivity, contraction and compatibility with the service environment. Cryogenic testing uses temperature control and appropriate strain measurement, rather than assuming that room-temperature data remain valid.

Visual 5.10
An environmental chamber and suitable instrumentation support low-temperature mechanical testing. Illustrative view.

39. Ductile-to-brittle transition and impact energy

Many ferritic BCC steels show a ductile-to-brittle transition as temperature falls. Plastic flow becomes more difficult relative to cleavage, and impact specimens can absorb much less energy. Notch severity, strain rate, grain size, composition and material condition influence the transition behaviour.

A transition temperature is defined by a chosen criterion, such as a specified absorbed energy or fracture appearance. Different criteria need not give the same temperature. Charpy impact energy is also not identical to fracture toughness; the tests describe different responses.

Figure 5.38
Schematic impact-energy transition; its temperature depends on material condition and the chosen criterion.

The sigmoid curve in the figure is a schematic trend, not certified data for a named steel. Read a supplied dataset using the stated criterion. Finer grains and suitable processing can improve transition behaviour, but a universal safe minimum temperature cannot be assigned from crystal structure alone.

40. Low-temperature material selection

Selected austenitic stainless steels, aluminium alloys and copper alloys often retain useful ductility at low temperature. This is one reason they are considered for many cryogenic components. The exact alloy, weld condition and service requirements still determine suitability.

Avoid the rule that every FCC material is automatically acceptable or every HCP material is brittle. Some carefully selected titanium alloys can perform well at cryogenic temperatures. Ferritic steels need particular attention to transition behaviour, while polymers and elastomers can stiffen or lose sealing performance near their glass-transition range.

Figure 5.39
Low-temperature selection balances load support, crack tolerance, contraction and heat transfer.

Ceramics remain brittle and can be sensitive to thermal shock; composites can suffer interface stresses from mismatched contraction. A complete selection compares mechanical response, contraction, heat transfer, joining and environmental compatibility. The final choice should use temperature-specific property evidence for the actual component condition.

Material family Key low-temperature check
Ferritic steel Transition and crack tolerance
Austenitic stainless / Al / Cu Grade, weld and toughness data
Polymers / seals Stiffening and glass transition
Composites / ceramics Mismatch and thermal shock

41. Thermal contraction and differential movement

For a small interval with a supplied constant expansion coefficient, free length change is ΔL = α L0 ΔT. Cooling gives a negative ΔT and hence contraction when α is positive. For a wide cryogenic interval, α varies with temperature; use integrated contraction data when supplied.

If two joined materials contract differently, their mismatch can produce interface forces, distortion or loss of seal contact. The free mismatch is a geometric estimate, not automatically the stress in a real assembly. Actual stresses depend on stiffness, joint geometry, constraints and plastic relaxation.

Figure 5.40
Supplied constant-coefficient examples show different free contractions; wide-range real coefficients may vary.

A fully restrained uniform bar with constant elastic properties gives σ = -E α ΔT under the ideal one-dimensional model. Cooling would therefore generate tension in that ideal restraint. Real cryogenic supports often use flexible details to accommodate movement rather than relying on the fully restrained-bar assumption.

42. Testing and inspection at low temperature

Low-temperature mechanical tests need an equilibrated specimen temperature and suitable instrumentation. Temperature gradients, grip conditions and extensometer response can influence the apparent result. Record the temperature and conditioning arrangement along with the mechanical measurement.

Inspection performance can also change with temperature. Couplants, adhesives, cables and sensors must be suitable for the operating range. Condensation or frost can obstruct visual inspection and affect contact. An instrument calibrated under unrelated conditions may need a qualified correction or a different examination arrangement.

Material behaviour during thermal cycling can be as important as behaviour after steady cooling. Examine seals, joints and interfaces as well as the bulk metal. The purpose is to connect the inspection with the likely failure mechanism, not to assume that one successful room-temperature examination proves cryogenic reliability.

43. High-temperature properties and microstructure

As temperature rises, elastic modulus and yield strength generally decrease for many structural metals, while diffusion-driven processes become faster. Short-term tensile behaviour, long-term creep resistance and environmental durability must be evaluated separately.

Recovery, recrystallisation, grain growth and precipitate coarsening can change properties during exposure. A heat-treated alloy may therefore evolve in service even if it never melts. Oxidation or hot corrosion can reduce section or damage protective surfaces in a suitable environment.

Figure 5.41
Schematic decreasing modulus and yield-strength trends; use grade-specific data for numerical design.

A material with high melting temperature is not automatically the best hot-service choice. Phase stability, oxidation resistance, density, manufacturability and thermal stress matter. Use the actual operating time-temperature history and material condition when discussing performance, and distinguish bulk temperature from a potentially hotter local surface.

44. Oxidation, coatings and loss of section

At high temperature, a surface oxide can either slow further reaction or fail to provide an effective barrier. Scale adherence, growth stresses, thermal cycling and environmental chemistry influence whether protection persists. Flaking or cracking can expose fresh metal.

For a supplied parabolic-growth model, x^2 = kp t after the stated reference condition. Thickness then increases with the square root of time. Some systems follow different kinetics or change regime, so the relation is not a universal law for every metal and atmosphere.

Figure 5.42
An assigned parabolic model makes scale thickness proportional to the square root of time.

Coatings and alloy additions can improve environmental resistance but must remain compatible with the substrate and service cycles. Mechanical damage or interdiffusion can affect performance. Wall-thickness loss changes the mechanical stress as well as the chemical condition, linking oxidation with creep and fracture assessment.

45. Thermal stress and thermal fatigue

Uniform free heating produces expansion without stress in an ideal unconstrained body. Stress develops when expansion is restrained or when temperature differences make neighbouring regions deform incompatibly. Rapid heating and cooling can therefore create severe local stresses.

A surface may heat or cool faster than the interior. Repeated gradients can generate cyclic plasticity and thermal-fatigue cracks. The sign and distribution of stress depend on geometry and the heating history; they cannot be inferred from temperature alone.

Figure 5.43
Different surface and interior temperature histories create incompatible strains and cyclic stresses.

Reducing thermal gradients, avoiding sharp geometric changes and permitting controlled movement can improve performance. High thermal conductivity and suitable expansion behaviour may be beneficial, but the selection must also satisfy strength, environment and manufacturing needs. Combine a thermal explanation with the expected crack location when answering an application question.

46. Materials for elevated-temperature service

Creep-resistant steels, nickel-based superalloys, selected ceramics and appropriate composites serve different hot-service roles. Stable precipitates, solid-solution strengthening and controlled grain structures can improve metal performance. Ceramic materials can offer high-temperature capability but may be limited by brittleness or thermal shock.

Directional or single-crystal structures can reduce grain-boundary-related deformation in particular turbine applications. They do not eliminate all creep, oxidation or fatigue. A coating can protect a surface while the substrate still carries the mechanical load.

Figure 5.44
Hot-service performance depends on stable structure, environmental resistance and thermal management.

Choose a material by the required temperature, stress, exposure time, environment, thermal cycling and acceptable deformation. Cooling and component design may be as influential as alloy selection. A statement such as use a superalloy should therefore be supported by the relevant mechanism and a realistic service requirement.

47. Hot-service inspection and condition monitoring

Inspection of a hot component requires equipment and a procedure suitable for its temperature and access. Sound velocity, probe response and couplant behaviour can change with temperature. An apparent thickness change may partly reflect an inappropriate calibration rather than real wall loss.

Monitoring can combine temperature history, dimensional measurements, surface inspection and relevant volumetric or microstructural examinations. Each method answers a different question: distortion, cracking, section loss, phase condition or active damage. A trend is meaningful only when successive measurements are comparable.

Do not infer safe remaining life from a single clean image. Conversely, do not treat every surface stain as a structural crack. Interpret the observation against service history, expected mechanisms and acceptance requirements. The strongest answer connects method selection, measured evidence and a justified follow-up action.

48. Method-selection examples across engineering parts

For an accessible steel lifting component, begin with visual examination for distortion, wear and surface condition. A suitable magnetic-particle examination may help investigate surface cracks. The load path and relevant acceptance requirements determine what an indication means.

For an aluminium aircraft-type panel, eddy-current testing can examine a fastener region with an appropriate reference and probe. Penetrant testing can help with accessible surface-connected features on a suitably prepared nonporous surface. Magnetic-particle testing is not the correct conventional choice for aluminium.

For a thick weld, choose UT or radiography according to geometry, likely discontinuity orientation and required coverage; surface methods may supplement them. For a phase-change question in a heat-treated sample, XRD is a more direct choice. These are selection principles, not a substitute for a qualified component-specific examination plan.

49. Common mistakes and the correction strategy

Do not use Celsius in homologous-temperature or activation-energy equations. Do not call a constant-load test a constant-true-stress test. Keep creep strain, total strain, strain rate and rupture time as separate quantities with clearly stated units.

For NDT, remember the physical requirement: penetrant needs a surface opening and suitable nonporosity; magnetic particles need ferromagnetism; eddy currents need conductivity. UT time is commonly a round trip, and angle-beam sound path differs from normal depth. AE listens for active sources rather than sending a standard pulse.

Radiography is an attenuation projection; diffraction concerns crystal planes. Halve a reported 2θ angle before using Bragg law. At low temperature, increased strength does not necessarily mean increased toughness. In every answer, state the mechanism, draw the relevant geometry and identify the limit of the conclusion.

50. How to construct a complete examination answer

Begin with a precise definition and identify the controlling physical mechanism. A method answer should then show the labelled component, source or probe, signal path and observation. Name the materials or discontinuities for which the method is appropriate.

Describe the operating sequence as separate numbered steps rather than one dense paragraph. Include interpretation and limitations: a response must be evaluated, and a missing signal has several possible causes. Where a relation is used, define every symbol and state the assumed geometry and units.

Finish with an application and a reason for choosing the method. For a numerical question, show conversions, substitution, result and a physical check. The worked problems and revision section apply this structure using original teaching questions; examination-year questions will be added separately.

WORKED PROBLEMS AND INSPECTION CASES

Numerical values are original teaching inputs. State units, geometry and the supplied model. Inspection cases explain method selection and interpretation; the observations must still be evaluated against component-specific requirements.

Worked problem 5.1: Average secondary creep rate

A specimen accumulates 0.24% additional creep strain between 200 h and 800 h. Find its average rate in h^(-1) and s^(-1).

  • 1. Convert strain: 0.24% = 0.0024. The elapsed interval is 800 – 200 = 600 h.

  • 2. Rate = 0.0024/600 = 4.00 × 10^(-6) h^(-1).

  • 3. Divide by 3600 to convert the hourly rate into a rate per second.

Answer. 4.00 × 10^(-6) h^(-1), or 1.11 × 10^(-9) s^(-1).

Check. Use the interval, not the final clock reading; a percent is not a unit strain.

Worked problem 5.2: Norton stress-rate ratio

At unchanged temperature, creep rate follows A σ^4 over the stated range. What happens when stress increases from 80 MPa to 100 MPa?

  • 1. Form the ratio so that the unchanged coefficient cancels.

  • 2. Rate2/rate1 = (100/80)^4 = 1.25^4.

  • 3. Evaluate the dimensionless power.

Answer. The predicted rate increases by a factor of 2.44.

Check. The stress increases by 25%, but the rate increases by about 144%; the law applies only in its supplied range.

Worked problem 5.3: Temperature acceleration of creep

At fixed stress, use an activation energy Q = 180 kJ mol^(-1) to estimate the rate ratio between 800 K and 850 K. Take R = 8.314 J mol^(-1) K^(-1).

  • 1. Convert Q = 180000 J mol^(-1).

  • 2. Exponent = (180000/8.314)(1/800 – 1/850) = 1.592.

  • 3. Rate at 850 K / rate at 800 K = exp(1.592).

Answer. Rate ratio ≈ 4.91.

Check. The higher temperature must give the higher rate in this supplied thermally activated model.

Worked problem 5.4: Fatigue cycle quantities

A load cycle has maximum stress 150 MPa and minimum stress -50 MPa. Find amplitude, mean stress, range and stress ratio.

  • 1. Stress amplitude = [150 – (-50)]/2 = 100 MPa.

  • 2. Mean stress = [150 + (-50)]/2 = 50 MPa. Stress range = 200 MPa.

  • 3. Stress ratio R = -50/150 = -0.333.

Answer. Amplitude 100 MPa; mean 50 MPa; range 200 MPa; R = -0.333.

Check. The cycle is partly compressive and has a tensile mean; amplitude is half the range.

Worked problem 5.5: Normal-beam ultrasonic depth

A delay-corrected reflector echo returns after 8.0 µs in steel. Use longitudinal velocity 5900 m s^(-1). Find reflector depth.

  • 1. Convert time: 8.0 µs = 8.0 × 10^(-6) s.

  • 2. The pulse travels out and back: d = ct/2.

  • 3. d = 5900 × 8.0 × 10^(-6)/2 = 0.0236 m.

Answer. Reflector depth = 23.6 mm.

Check. Using ct without the factor of two would give the full round-trip path, 47.2 mm.

Worked problem 5.6: Angle-beam sound path and coordinates

A first-leg echo has corrected time 20 µs. Shear-wave velocity is 3200 m s^(-1), and the refracted angle is 60° from the surface normal. Find sound path, depth and offset.

  • 1. One-way sound path s = ct/2 = 3200 × 20 × 10^(-6)/2 = 0.032 m = 32 mm.

  • 2. Normal depth z = s cos 60° = 16.0 mm.

  • 3. Surface projection x = s sin 60° = 27.7 mm.

Answer. Sound path 32.0 mm; depth 16.0 mm; horizontal offset 27.7 mm.

Check. The geometry assumes no back-wall reflection; the angle is in the material and measured from the normal.

Worked problem 5.7: AE source location with a signed delay

Sensors are 1.2 m apart on a straight bar. Direct wave speed is 3000 m s^(-1). The right sensor receives an event 100 µs after the left. Find x from the left.

  • 1. Use Δt = tright – t_left = +100 × 10^(-6) s.

  • 2. Distance difference cΔt = 3000 × 100 × 10^(-6) = 0.300 m.

  • 3. x = (L – cΔt)/2 = (1.2 – 0.3)/2.

Answer. The source is 0.450 m from the left sensor.

Check. Left and right travel times are 150 µs and 250 µs; their difference is the stated 100 µs.

Worked problem 5.8: Radiographic geometric unsharpness

Effective source size is 2 mm. Source-to-object distance a = 600 mm and object-to-detector gap b = 30 mm. Calculate Ug.

  • 1. Use Ug = F b/a with all lengths in the same units.

  • 2. Ug = 2 × 30/600 mm.

  • 3. If the gap is reduced to 10 mm with the other quantities unchanged, repeat the calculation.

Answer. Ug = 0.100 mm; reducing the gap to 10 mm gives 0.0333 mm.

Check. This covers geometric unsharpness only, not detector blur, motion or all image-quality effects.

Worked problem 5.9: Bragg spacing from a 2θ peak

A first-order peak occurs at 2θ = 60°. Wavelength is 0.154 nm. Find interplanar spacing d.

  • 1. Halve the plotted angle: θ = 30°. Use n = 1.

  • 2. From nλ = 2d sin θ, d = 0.154/[2 sin 30°] nm.

  • 3. Since sin 30° = 0.5, evaluate the spacing.

Answer. Interplanar spacing d = 0.154 nm.

Check. Substituting 60° as θ would incorrectly give about 0.0889 nm.

Worked problem 5.10: Differential contraction of joined materials

Two free 500 mm members cool by 200 K. Supplied constant coefficients are 12 × 10^(-6) K^(-1) and 23 × 10^(-6) K^(-1). Find their free contractions and mismatch.

  • 1. ΔT = -200 K. First length change = 12 × 10^(-6) × 500 × (-200) = -1.20 mm.

  • 2. Second length change = 23 × 10^(-6) × 500 × (-200) = -2.30 mm.

  • 3. Difference in free contraction magnitudes = 2.30 – 1.20 = 1.10 mm.

Answer. Free contractions are 1.20 mm and 2.30 mm; mismatch magnitude is 1.10 mm.

Check. These are free movements. Joint stresses need stiffness and constraint data; wide-range real coefficients can vary with temperature.

QUICK REVISION: QUESTIONS WITH ANSWERS

Is a brittle fracture always a low-strength event?

No. Brittle response describes limited macroscopic plastic deformation and the crack-growth mechanism, not a universal low strength. Constraint, temperature, loading rate and defects affect fracture behaviour.

Indication, discontinuity or defect?

An indication is a response; a discontinuity is a structural interruption; a defect fails applicable acceptance requirements. Evaluation must connect the observation with the component and its governing criteria.

Why is magnetic-particle testing unsuitable for aluminium?

The method requires ferromagnetism to establish the relevant magnetic flux and leakage response. Aluminium is conductive but not ferromagnetic. Conductivity alone does not make it suitable for MT.

Is higher UT frequency always better?

No. Shorter wavelength may improve resolution, but attenuation and grain scattering can increase. Material, thickness, geometry and the required sensitivity determine a suitable frequency.

How is acoustic emission different from UT?

AE listens for energy released by active sources within the material. UT usually transmits a known pulse and observes reflections or transmission. A dormant discontinuity may remain silent in AE.

Why can cryogenic strength increase while toughness decreases?

Resistance to plastic flow and resistance to crack extension are different properties. Some steels become less able to accommodate notch stresses at low temperature and show transition behaviour despite increased tensile strength.

FORMULAS AND DECISION QUICK REFERENCE

Quantity / model Relation and essential condition
Total strain / extension εtotal = εinitial + εcreep; ΔL = L0 ε for the stated engineering-strain basis.
Average creep rate Rate = Δε/Δt; percent strain ÷ 100; hours × 3600 = seconds.
Steady-rate interval Additional ε = rate × time; excludes unmodelled tertiary acceleration.
Homologous temperature TH = T/Tm; use kelvin in both terms.
True / engineering stress Current true stress = F/Acurrent; engineering stress = F/A0.
Norton ratio Rate2/rate1 = (σ2/σ1)^n at fixed temperature in the supplied regime.
Thermally activated ratio Rate2/rate1 = exp[(Q/R)(1/T1 – 1/T2)] at fixed stress and unchanged model.
Time-temperature parameter P = T(C + log10 tr); use the supplied C, temperature and time units.
Fatigue cycle σa = (σmax – σmin)/2; σm = (σmax + σmin)/2; R = σmin/σmax.
UT pulse-echo Normal depth d = ct/2 after delay correction; one-way sound path s = ct/2.
Angle-beam first leg z = s cos θ; x = s sin θ; θ measured from surface normal.
Wavelength λ = c/f; use the correct wave-mode velocity.
AE bar localisation x = (L – cΔt)/2; Δt = right arrival minus left arrival; constant direct-path speed.
Ideal attenuation I/I0 = exp(-μx); monoenergetic narrow-beam model, matching μ and x units.
Geometric unsharpness Ug = F b/a; a = source-object distance; b = object-detector gap.
Bragg law nλ = 2d sin θ; halve a reported 2θ angle before substitution.
Directional lattice strain ε = (d – d0)/d0 for the same indexed reflection and suitable stress-free reference.
Ideal skin depth δ = 1/√(π f μ σ); SI units; amplitude at δ is 1/e of surface value.
Free thermal movement ΔL = α L0 ΔT for supplied constant α; use integrated data over wide ranges.
Ideal restrained bar σ = -E α ΔT for fully restrained uniform uniaxial elastic response with constant properties.
Parabolic oxide growth x² = kp t from the stated origin; x2/x1 = √(t2/t1) under the same model.

PYQs WITH ANSWERS – UNIT V

Questions from the five supplied papers, grouped by examination year, with original numbers, marks and answers. Labelled sketches accompany the questions that require them.

Marks Theory target What to include
2 40-60 words Direct definition or requested points; a formula or example where useful.
7 150-200 words A short introduction, organised explanation or comparison, and a relevant sketch.
10 250-300 words A complete structured explanation, key distinctions and a relevant example, table or diagram.

Writing guide: These are practical targets, not prescribed AKTU word limits. Follow the exact question. For numericals, show given data, assumptions, formula, substitution, units and the final result; do not add prose just to meet a word count.

Legacy coverage: stress-intensity, Griffith fracture and static failure-theory questions from older KME303 papers are included here as failure-related extensions; their original unit arrangement differs from the current syllabus.

EXAMINATION 2021-22 | KME303

Q1 (2021-22)

Original Q1(c) | Section A | 2 marks | Legacy extension

Explain Stress intensity factor.

Answer

The stress-intensity factor K describes the intensity of a crack-tip elastic stress field for a specified loading mode. For a common Mode I geometry, KI = Yσ√(πa), where Y accounts for geometry and a is the defined crack dimension. Its units are MPa√m. Compare it with the appropriate fracture toughness to assess crack extension.

Q2 (2021-22)

Original Q2(b) | Section B | 10 marks | Legacy extension

Discuss following theories of failure in brief: (1) Maximum principal stress theory (2) Maximum shear stress Theory (3) Maximum distortion energy theory.

Answer

  • 1. Scope. Static failure criteria compare a multiaxial stress state with material limits. For a ductile metal, the usual comparison predicts initial yielding, not complete fracture. Brittle fracture can require different tensile/compressive limits and crack-based analysis.

  • 2. Maximum principal stress: Rankine. Failure is associated with a principal normal stress reaching its relevant uniaxial limit. Compare the largest tensile principal stress with tensile strength and the most compressive stress with the appropriate compressive limit. It is not a general ductile-yield model.

  • 3. Maximum shear stress: Tresca. Order principal stresses σ1 ≥ σ2 ≥ σ3. Maximum shear stress is (σ1 – σ3)/2. In uniaxial tension at yield it is σy/2, so the yield condition is σ1 – σ3 = σy.

  • 4. Maximum distortion energy: von Mises. Define σvm = √{[(σ1 – σ2)² + (σ2 – σ3)² + (σ3 – σ1)²]/2}. Initial yield is predicted when σvm reaches the uniaxial yield stress.

  • 5. Comparison. For pure shear, Tresca predicts τy = σy/2 and von Mises predicts τy = σy/√3. Both ideal isotropic ductile-yield criteria are insensitive to an added equal hydrostatic stress, unlike a simple principal-stress rule.

  • 6. Use. Select a criterion appropriate to the material and failure mode, apply a stated design factor if required and do not equate first yield with fatigue life, creep rupture or crack instability.

  • 7. For example, in a plane-stress state with principal stresses 100, 40 and 0 MPa, the Tresca equivalent stress is 100 MPa and von Mises equivalent stress is √7600 ≈ 87.2 MPa. The difference illustrates the criterion choice; a verdict still requires a specified material limit.

Figure 5.45
PYQ diagram 5.1. Normalised plane-stress yield boundaries for Tresca and von Mises.

Q3 (2021-22)

Original Q4(a) | Section C | 10 marks | Legacy extension

Explain Griffith theory for brittle fracture and formulate the expression for critical crack size.

Answer

  • 1. Physical idea. A crack can extend when release of elastic strain energy supplies the energy needed to create new crack surfaces. Griffith’s ideal treatment explains why a brittle solid with a crack can fail far below its perfect-lattice strength.

  • 2. Geometry and assumptions. Consider a central through-crack of total length 2a in a large plate under remote Mode I tensile stress σ. Assume linear elasticity, a sharp crack and negligible plastic dissipation. Define γs as surface energy per unit newly created surface area.

  • 3. Energy release. For the ideal infinite-plate geometry, the energy release rate is G = πaσ²/E′. Here E′ = E for plane stress and E/(1 – ν²) for plane strain.

  • 4. Critical condition. Two new surfaces require Gc = 2γs. Setting G = Gc gives σc = √[2E′ γs/(πa)]. A larger crack therefore requires a lower remote stress for extension under the same assumptions.

  • 5. Critical crack size. Rearranging gives the critical half-length ac = 2E′ γs/(πσ²). The corresponding full crack length is 2ac = 4E′ γs/(πσ²). State clearly which length is requested.

  • 6. Engineering extension. Real materials can dissipate energy through plasticity and other mechanisms, so measured fracture resistance replaces surface energy alone. For finite geometry use KI = Yσ√(πa) and the appropriate toughness criterion; do not insert Y = 1 without checking the geometry.

  • 7. Unit check: E′ γs/σ² has units of length because γs is J/m² = N/m. The model addresses crack extension, not the time required for fatigue growth. Surface energy and fracture toughness are different quantities and cannot be substituted without the corresponding relation.

Figure 5.46
PYQ diagram 5.2. Central crack: a is the half-length and loading opens the crack.

Q4 (2021-22)

Original Q4(b) | Section C | 10 marks

Discuss the fatigue failure and method of developing S-N curve for steel using RR Moore test.

Answer

  • 1. Fatigue mechanism. Cyclic loading can initiate cracks at surface marks, notches, inclusions or other stress concentrators. A crack then grows over many cycles before the remaining section fails by final overload. Nominal stress can remain below monotonic yield.

  • 2. Rotating-bending principle. In an R.R. Moore-type test, a specimen rotates under a controlled bending moment. A point at the outer surface passes through tensile and compressive stress on each revolution. Under the ideal constant-moment arrangement, this is fully reversed loading with mean stress zero and R = -1.

  • 3. Procedure. Prepare comparable specimens and control dimensions, surface finish, alignment and environment. Apply a chosen bending-stress amplitude, run the machine and count cycles until the defined failure or runout criterion.

  • 4. Develop the curve. Repeat at several stress amplitudes with suitable replicate tests. Plot amplitude S vertically and cycles N on a logarithmic horizontal axis. Record nonfailed runouts distinctly rather than plotting them as actual failures.

  • 5. Steel trend. Some steels exhibit a long-life endurance-limit behaviour under particular laboratory conditions. This is not a universal limit for all steels, notches or environments. Surface, size, reliability and mean-stress effects matter for components.

  • 6. Conclusion. The experiment supplies an S-N relationship for the stated loading and specimen condition. It does not directly predict creep life or the growth of every pre-existing crack.

Figure 5.47
PYQ diagram 5.3. Rotating bending alternates tension and compression at an outer-surface point.
Figure 5.48
PYQ diagram 5.4. S-N data must specify amplitude, cycle criterion and test condition.

EXAMINATION 2022-23 | KME-303

Q5 (2022-23)

Original Q1(c) | Section A | 2 marks

What do you mean by Fatigue? Explain.

Answer

Fatigue is progressive damage under repeated or fluctuating stress, often involving crack initiation, gradual growth and final fracture of the remaining section. It can occur below the monotonic yield strength. Stress amplitude, mean stress, cycles, surface condition, notches and environment affect fatigue performance; a single static-strength value does not establish fatigue life.

Q6 (2022-23)

Original Q1(d) | Section A | 2 marks

Explain Non-Destructive Testing.

Answer

Non-destructive testing examines material or component condition without intentionally impairing its intended use. Examples include visual, penetrant, magnetic-particle, ultrasonic and radiographic testing. Each responds to particular physical features and has limitations. An indication must be interpreted and evaluated against applicable requirements; NDT does not prove complete absence of every possible discontinuity.

Q7 (2022-23)

Original Q2(b) | Section B | 10 marks

Elaborate the ductile and brittle failure mechanism.

Answer

  • 1. Ductile failure. Considerable local plastic deformation can occur before fracture. Microvoids nucleate around particles or inclusions, grow and coalesce. A tensile specimen can show necking and a cup-and-cone appearance; microscopic dimples provide additional evidence.

  • 2. Brittle failure. Crack growth occurs with limited macroscopic plastic deformation. Cleavage can proceed across grains, while intergranular fracture follows weakened boundaries. The observed mechanism depends on material condition and environment.

  • 3. Stress-state effect. Notches and high constraint reduce the ability to accommodate a crack-tip stress concentration. Low temperature or high loading rate can increase brittle susceptibility in certain steels. A material that is ductile in one test need not behave identically in every geometry.

  • 4. Energy and evidence. Ductile tensile failure commonly absorbs more deformation energy, while brittle failure can be rapid with little visible warning. Fracture toughness is a crack-resistance property and must not be replaced by tensile strength or a visual judgement alone.

  • 5. Investigation. Locate initiation, growth and final overload regions and connect them to the service history. A fatigue crack may finish with a ductile overload region, so the final appearance does not necessarily identify the whole event.

  • 6. Sketch. Label necking, void linkage or cup-and-cone features for a typical ductile case and a relatively low-plasticity crack plane for a brittle case. State that these are characteristic examples rather than universal appearances.

Feature Ductile Brittle
Plastic deformation Often substantial locally Limited macroscopically
Typical mechanism Void growth / coalescence Cleavage or boundary fracture
Usual visible clue Necking may occur Little necking
Figure 5.49
PYQ diagram 5.5. Typical ductile necking and limited-plasticity fracture geometry.

Q8 (2022-23)

Original Q4(a) | Section C | 10 marks | Legacy extension

Name the various types of Static Failure Theories. Explain any one in detail.

Answer

  • 1. Common theories. Introductory static criteria include maximum principal stress, maximum principal strain, maximum shear stress, maximum total strain energy, maximum distortion energy and suitable Mohr-type criteria. Their physical suitability and required material strengths differ.

  • 2. Explain von Mises in detail. Elastic strain energy can be separated into volumetric and distortional parts. The von Mises criterion associates initial yielding of an ideal isotropic ductile metal with the distortional contribution reaching that of a uniaxial test at yield.

  • 3. Equivalent stress. In principal stresses, σvm = √{[(σ1 – σ2)² + (σ2 – σ3)² + (σ3 – σ1)²]/2}. Compare σvm with the specified yield stress σy. Under plane stress, the full expression still includes the third principal stress, which is zero.

  • 4. Special cases. Uniaxial tension gives σvm = |σ|. Pure shear gives σvm = √3|τ| and hence τy = σy/√3. Equal hydrostatic stresses give zero von Mises equivalent stress under this ideal yield model.

  • 5. Interpretation. The criterion predicts first yield, not a fracture location or crack-growth life. Brittle materials and pressure-sensitive behaviour can require a different approach.

  • 6. Comparison. Tresca uses maximum shear and can be more conservative in parts of the principal-stress plane. Present the criterion, its assumptions, a labelled envelope and a consistent strength comparison rather than listing names alone.

Figure 5.50
PYQ diagram 5.6. Two common ideal ductile-yield criteria.

Q9 (2022-23)

Original Q4(b) | Section C | 10 marks

Discuss the SN Curve in detail. Explain typical S-N curve for ferrous and non-ferrous alloys.

Answer

  • 1. Definition and axes. An S-N curve relates a stated cyclic stress measure, commonly amplitude, to cycles to a defined failure criterion. N is normally plotted logarithmically. Specify mean stress, stress ratio, specimen and environment.

  • 2. How data are obtained. Test comparable specimens at several controlled stress amplitudes and record cycles to failure or runout. Fatigue scatter means that one specimen at each level does not establish a universal deterministic life.

  • 3. Ferrous trend. Some steels show a knee followed by approximately limiting long-life strength under particular laboratory conditions. The associated endurance limit must be qualified by the test condition, surface and environment.

  • 4. Nonferrous trend. Many aluminium and other nonferrous alloys show a continuing decrease in fatigue strength with increasing cycles over the tested range. Their fatigue strength is therefore commonly specified at a chosen number of cycles.

  • 5. Mechanism and influences. Initiation and propagation depend on stress concentrations, surface finish, residual stress, size, mean stress and corrosion. A crack can grow at nominal stresses below the monotonic yield strength.

  • 6. Correct comparison. The categories describe common trends rather than an absolute rule that all ferrous materials have an endurance limit and all other materials behave identically. Mark runouts and the actual stress measure, and do not use an amplitude curve with stress range without the factor-of-two conversion.

Figure 5.51
PYQ diagram 5.7. Illustrative limiting and continuously falling long-life trends.

EXAMINATION 2023-24 | BME303

Q10 (2023-24)

Original Q1(g) | Section A | 2 marks

Define the term fatigue strength.

Answer

Fatigue strength is the stress level associated with a specified number of cycles and defined loading, environment and failure criterion. State whether stress is amplitude, range or maximum. It is different from an endurance limit, which describes limiting long-life behaviour only for materials and conditions that exhibit it.

Q11 (2023-24)

Original Q2(e) | Section B | 7 marks

Differentiate between ductile failure and brittle failure. Also explain fracture mechanism with neat diagram.

Answer

  • 1. Ductile failure. Considerable local plastic deformation can occur before fracture. Microvoids nucleate around particles or inclusions, grow and coalesce. A tensile specimen can show necking and a cup-and-cone appearance; microscopic dimples provide additional evidence.

  • 2. Brittle failure. Crack growth occurs with limited macroscopic plastic deformation. Cleavage can proceed across grains, while intergranular fracture follows weakened boundaries. The observed mechanism depends on material condition and environment.

  • 3. Stress-state effect. Notches and high constraint reduce the ability to accommodate a crack-tip stress concentration. Low temperature or high loading rate can increase brittle susceptibility in certain steels. A material that is ductile in one test need not behave identically in every geometry.

  • 4. Energy and evidence. Ductile tensile failure commonly absorbs more deformation energy, while brittle failure can be rapid with little visible warning. Fracture toughness is a crack-resistance property and must not be replaced by tensile strength or a visual judgement alone.

  • 5. Investigation. Locate initiation, growth and final overload regions and connect them to the service history. A fatigue crack may finish with a ductile overload region, so the final appearance does not necessarily identify the whole event.

  • 6. Sketch. Label necking, void linkage or cup-and-cone features for a typical ductile case and a relatively low-plasticity crack plane for a brittle case. State that these are characteristic examples rather than universal appearances.

Feature Ductile Brittle
Plastic deformation Often substantial locally Limited macroscopically
Typical mechanism Void growth / coalescence Cleavage or boundary fracture
Usual visible clue Necking may occur Little necking
Figure 5.52
PYQ diagram 5.8. Typical ductile necking and limited-plasticity fracture geometry.

Q12 (2023-24)

Original Q7(a) | Section C | 7 marks

Explain creep failure. Also explain creep curve with creep mechanism.

Answer

  • 1. Definition. Creep is progressive time-dependent deformation under sustained stress or load. Temperature, stress, microstructure, composition and environment influence its rate. A metal’s short-term yield strength is insufficient for long-duration hot-service assessment.

  • 2. Primary stage. After the instantaneous loading strain, the creep rate commonly decreases as deformation resistance develops. The strain-time curve continues rising, but its slope becomes smaller.

  • 3. Secondary stage. An approximate balance of hardening and recovery produces a near-minimum, approximately steady rate over a useful interval. Dislocation glide/climb or diffusion-related mechanisms can contribute, depending on the regime.

  • 4. Tertiary stage. Cavitation, boundary damage, crack linkage and section reduction can accelerate deformation towards rupture. In a constant-load test, decreasing current area also raises true stress.

  • 5. Mechanisms. Diffusion-assisted dislocation climb helps bypass obstacles. Lattice and grain-boundary diffusion can support diffusion creep under suitable conditions; grain-boundary sliding and damage accommodation can also matter.

  • 6. Interpretation. Draw total strain versus time with the loading strain and three typical regions. Distinguish slope/rate from accumulated strain and a distortion criterion from rupture time. Not every material displays three sharply separated stages, and a steady-rate estimate cannot represent unmodelled tertiary acceleration.

Figure 5.53
PYQ diagram 5.9. Typical strain-time stages; slopes give creep rates.
Figure 5.54
PYQ diagram 5.10. Creep cavities can link into cracks during damage evolution.

Q13 (2023-24)

Original Q7(b) | Section C | 7 marks

Discuss Ultra Sonic test and Magnetic Particle Test in case of Non-Destructive Test.

Answer

  • 1. Ultrasonic principle. A transducer introduces elastic waves and receives suitable reflections. In conventional contact pulse-echo testing, couplant improves acoustic transfer into the part. Calibrated echo time helps locate a reflector; for a normal beam, depth is ct/2 after delay correction.

  • 2. UT use and limits. Welds, forgings and thickness measurements are common applications. One-sided access can be useful, but velocity, wave mode, coupling, grain scattering and reflector orientation affect response. An echo is not a direct photograph or a universal size measurement.

  • 3. Magnetic-particle principle. Magnetise a ferromagnetic component. A suitable surface or near-surface discontinuity disturbs flux and creates leakage, causing particles to form an indication. A field crossing the crack generally gives a stronger response than a parallel field.

  • 4. MT use and limits. Steel shafts, selected welds and other ferromagnetic parts are suitable examples. The method is relatively direct for accessible surface flaws but does not suit aluminium or ordinary austenitic stainless steel. Deep internal coverage is limited.

  • 5. Coverage and evaluation. Use adequate calibration/system checks, controlled scanning or magnetisation coverage and more than one field direction where required. Record location and evaluate relevant indications against the governing requirements; a missing response does not prove complete absence of every flaw.

Figure 5.55
PYQ diagram 5.11. Probe, couplant, reflector and returning echo.
Figure 5.56
PYQ diagram 5.12. Flux leakage and particle accumulation at a discontinuity.

EXAMINATION 2024-25 | BME303

Q14 (2024-25)

Original Q1(g) | Section A | 2 marks

Differentiate between NDT and destructive testing.

Answer

NDT examines a component without intentionally impairing its intended use, for example by UT or penetrant testing. Destructive testing deliberately loads, deforms, cuts or fractures a specimen to measure a property or response, as in tensile or impact testing. NDT indications and destructive-test property measurements provide different information and can complement each other.

Q15 (2024-25)

Original Q2(e) | Section B | 7 marks

What is Non-Destructive Testing (NDT)? Explain in detail any two NDT methods.

Answer

  • 1. Definition and selection. NDT examines condition without intentionally impairing intended use. Choose a technique by material, expected discontinuity, access and the required information. Penetrant and ultrasonic testing provide two distinct examples.

  • 2. Method 1: penetrant principle. A suitable wetting liquid enters surface-connected openings in a nonporous component. Developer draws retained liquid out after excess surface penetrant is removed, producing an indication.

  • 3. Penetrant sequence. Clean and dry, apply penetrant, allow the specified dwell, remove excess by the selected system, apply developer, inspect under the required viewing conditions, record and post-clean as required. Sealed internal defects are not detected and porous surfaces can give heavy background.

  • 4. Method 2: ultrasonic principle. A transducer introduces elastic waves and observes reflected signals. Conventional contact pulse-echo testing uses a couplant. With known velocity and corrected round-trip time, normal-beam reflector depth is ct/2.

  • 5. UT application and limits. Suitable welds, forgings and wall-thickness measurements can be examined. Coarse grains, geometry, near-surface effects and unfavourable reflector direction can reduce capability.

  • 6. Evaluation. A penetrant stain or ultrasonic echo is an indication requiring interpretation. Record location and coverage, distinguish nonrelevant responses and use the applicable acceptance requirements. No method proves a part is entirely discontinuity-free.

Figure 5.57
PYQ diagram 5.13. Penetrant preparation and development sequence.
Figure 5.58
PYQ diagram 5.14. A pulse-echo UT arrangement.

Q16 (2024-25)

Original Q7(a) | Section C | 7 marks

Explain the Material behavior at a very low (Cryogenics) and high temperature with the help of a stress-strain curve.

Answer

  • 1. Low-temperature response. Strength and stiffness can increase in many metals as temperature falls, but ductility and toughness can decrease in susceptible materials. Some ferritic BCC steels show a ductile-to-brittle transition. Increased strength must not be equated with increased crack tolerance.

  • 2. Cryogenic selection. Selected austenitic stainless steels, aluminium and copper alloys often retain useful ductility. Grade, weld condition, notch constraint and the actual temperature still matter. Thermal contraction, seals and differential movement also require attention.

  • 3. Stress-strain illustration. A susceptible steel can show a higher flow stress but much smaller fracture strain at low temperature. At elevated temperature, many metals show a lower elastic slope and lower short-term flow strength. The plotted curves are illustrative, not data for every metal.

  • 4. High-temperature time effects. Sustained loading can cause creep and eventual rupture. Diffusion, recovery, grain growth and precipitate evolution can change long-term properties. A rapid tensile curve alone does not capture years of exposure.

  • 5. Environment and thermal cycles. Oxidation, hot corrosion and section loss can interact with mechanical stress. Nonuniform or restrained heating produces thermal stress, and repeated gradients can cause thermal fatigue.

  • 6. Conclusion. Use temperature- and time-specific data for the actual material. Choose by strength, crack tolerance, contraction and environment together rather than room-temperature strength alone.

Figure 5.59
PYQ diagram 5.15. Illustrative temperature-dependent tensile response for a susceptible metal.
Figure 5.60
PYQ diagram 5.16. A separate impact-energy transition illustrates toughness changes.

Q17 (2024-25)

Original Q7(b) | Section C | 7 marks

Explain the term creep, its mechanism and stages.

Answer

  • 1. Definition. Creep is progressive time-dependent deformation under sustained stress or load. Temperature, stress, microstructure, composition and environment influence its rate. A metal’s short-term yield strength is insufficient for long-duration hot-service assessment.

  • 2. Primary stage. After the instantaneous loading strain, the creep rate commonly decreases as deformation resistance develops. The strain-time curve continues rising, but its slope becomes smaller.

  • 3. Secondary stage. An approximate balance of hardening and recovery produces a near-minimum, approximately steady rate over a useful interval. Dislocation glide/climb or diffusion-related mechanisms can contribute, depending on the regime.

  • 4. Tertiary stage. Cavitation, boundary damage, crack linkage and section reduction can accelerate deformation towards rupture. In a constant-load test, decreasing current area also raises true stress.

  • 5. Mechanisms. Diffusion-assisted dislocation climb helps bypass obstacles. Lattice and grain-boundary diffusion can support diffusion creep under suitable conditions; grain-boundary sliding and damage accommodation can also matter.

  • 6. Interpretation. Draw total strain versus time with the loading strain and three typical regions. Distinguish slope/rate from accumulated strain and a distortion criterion from rupture time. Not every material displays three sharply separated stages, and a steady-rate estimate cannot represent unmodelled tertiary acceleration.

Figure 5.61
PYQ diagram 5.17. Typical strain-time stages; slopes give creep rates.
Figure 5.62
PYQ diagram 5.18. Creep cavities can link into cracks during damage evolution.

EXAMINATION 2025-26 | BME303

Q18 (2025-26)

Original Q1(g) | Section A | 2 marks

Define creep? What are the different factors influence creep rate?

Answer

Creep is progressive time-dependent deformation under sustained load or stress. Rate depends on temperature, stress, alloy composition, microstructure, grain size, environment and prior exposure. At elevated temperature, dislocation motion, recovery and diffusion become important. Use kelvin in temperature ratios and thermally activated models; short-term yield strength alone does not describe long-term creep behaviour.

Q19 (2025-26)

Original Q2(e) | Section B | 7 marks

What is the difference between X-ray diffraction and radiography? Explain the process principle of X-ray diffraction used in NDT.

Answer

  • 1. Radiographic principle. Radiography forms a transmission projection: changes in thickness, density or composition alter attenuation between a source and detector. It can reveal suitable internal discontinuities, but superimposed features and planar-flaw orientation can limit interpretation.

  • 2. Diffraction principle. XRD measures constructive interference from regularly spaced crystal planes. For a reflection, nλ = 2d sin θ. The wavelength and diffraction angle therefore allow the corresponding plane spacing to be calculated.

  • 3. Arrangement and process. Direct an X-ray beam at a prepared crystalline specimen, scan an appropriate source/sample/detector geometry and record intensity against angle. Conventional powder patterns commonly use 2θ on the axis, so halve that value before using Bragg law.

  • 4. Applications. Multiple peaks and reference information support phase identification. Lattice-spacing changes can support strain studies; appropriate models and elastic constants are required to derive residual stress. Texture and peak-broadening analyses require their own assumptions.

  • 5. Difference. A radiograph is an attenuation image of projected component features; a diffraction pattern characterises ordered crystal structure. A diffraction peak is not a pore image, and one peak does not uniquely identify every phase.

  • 6. Example. For first order, λ = 0.154 nm and 2θ = 60° give θ = 30° and d = 0.154 nm. This illustrates the angle distinction rather than a measured phase assignment.

Figure 5.63
PYQ diagram 5.19. Radiography uses source-part-detector transmission.
Figure 5.64
PYQ diagram 5.20. Diffraction distinguishes θ from the scattering angle 2θ.

Q20 (2025-26)

Original Q7(a) | Section C | 7 marks

Discuss the working principle and applications of Magnetic Particle Inspection (MPI) and Ultrasonic Testing (UT) with suitable diagram. Enlist their advantages and disadvantages?

Answer

  • 1. UT working and applications. A transducer sends elastic pulses into a component and receives echoes. Conventional contact testing uses couplant. Normal-beam depth is ct/2 after instrument-delay correction. Weld examination and thickness measurements are common uses.

  • 2. UT advantages. Suitable arrangements can examine substantial thickness, use one-sided access and locate reflectors by travel time without a radiographic projection. Sensitivity can be high when the geometry and procedure are appropriate.

  • 3. UT disadvantages. Coupling, surface condition, attenuation, coarse grains, near-surface dead zones and unfavourable flaw orientation can limit the result. Calibration and skilled interpretation are needed; amplitude alone does not establish exact flaw dimensions.

  • 4. MPI working and applications. Magnetisation of a ferromagnetic part produces local leakage at suitably oriented discontinuities. Applied particles reveal an indication. Shafts, ferromagnetic weld regions and selected castings are examples.

  • 5. MPI advantages. It gives visible surface indications and can reveal some near-surface discontinuities. Local yoke arrangements can be practical for appropriate component geometry.

  • 6. MPI disadvantages. It requires ferromagnetism, has limited deep coverage and is sensitive to field direction and nonrelevant geometric effects. Surface preparation, adequate coverage and any required demagnetisation are important. Interpret both methods against the specified acceptance criteria.

Figure 5.65
PYQ diagram 5.21. Ultrasonic outgoing and return paths.
Figure 5.66
PYQ diagram 5.22. Magnetisation direction changes crack response.

Q21 (2025-26)

Original Q7(b) | Section C | 7 marks

How do metals behave at very low temperatures? Explain the effect of cryogenic temperatures on material properties. Discuss ductile-to-brittle transition temperature with examples.

Answer

  • 1. Definition and service range. Cryogenic service concerns very low temperatures; the actual operating range must be stated. Liquid-nitrogen and liquid-helium conditions are not interchangeable, and room-temperature property tables are insufficient.

  • 2. Mechanical effects. Many metals show increased flow strength as temperature falls, but susceptible steels can lose ductility and crack tolerance. Thermal contraction and differential movement can also affect joints and seals.

  • 3. Ductile-to-brittle transition. Many ferritic BCC steels show a marked change in impact energy and fracture appearance over a temperature range. At lower temperature, plastic accommodation becomes less effective relative to cleavage under the test conditions.

  • 4. Criterion and influencing factors. A transition temperature requires a specified criterion, such as an absorbed energy or fracture appearance. Grain size, composition, heat treatment, notch severity, thickness and loading rate affect it. Charpy energy is not identical to fracture toughness.

  • 5. Examples. Selected ferritic steels require careful transition assessment. Selected austenitic stainless steels, aluminium and copper alloys commonly retain useful low-temperature ductility. Some titanium alloys are also suitable; do not claim all HCP materials are brittle.

  • 6. Engineering conclusion. Verify grade, welds and actual service temperature, including contraction and cyclic loading. A strength increase does not independently demonstrate safe crack tolerance or justify a universal minimum temperature.

Figure 5.67
PYQ diagram 5.23. Schematic transition; its criterion and material condition must be specified.
←
Previous Story

Materials Engineering Unit 4 Notes – Heat Treatment and Surface Hardening of Steel

Next Story

Materials Engineering Notes – AKTU B.Tech Mechanical 2nd Year

→

Leave a Reply

Your email address will not be published. Required fields are marked *

Schedule Appointment

Fill out the form below, and we will be in touch shortly.
Contact Information
Vehicle Information
Preferred Date and Time Selection