Course Code: BME303
Course: AKTU B.Tech 2nd Year, Semester III
Unit: Crystal Structure and Mechanical Properties
Stream: Mechanical Engineering (ME)
Unit I Overview
Connect atomic arrangement and crystal imperfections with deformation, strengthening and measured properties. Study metallic structures and ceramics, slip and CRSS, tensile/compression/torsion tests, elastic laws, energy measures and hardness through labelled illustrations and worked examples.
Topics Covered
| Syllabus area | Pages |
|---|---|
| Crystal foundations | 2-6 |
| Ceramics and imperfections | 6-10 |
| Slip, CRSS and strengthening | 10-14 |
| Tension and stress-strain measures | 14-18 |
| Compression and torsion | 18-19 |
| Elastic constants and Hooke law | 19-20 |
| Energy and elastic recovery | 20-21 |
| Hardness and test interpretation | 21-24 |
| Worked problems | 24-27 |
| Quick revision checks | 27-28 |
| Formula quick reference | 29-29 |
| PYQs with Answers | 30-47 |
Learning Outcomes
- 1. Identify unit cells and calculate packing and density.
- 2. Explain defect classes, slip and strengthening.
- 3. Interpret tensile, compression and torsion results.
- 4. Apply isotropic elasticity and energy relations.
- 5. Compare hardness methods and their limits.
Included in These Notes
50 explained sections; 34 core diagrams and charts; 10 realistic illustrative images; 16 solved problems; comparison tables; 8 concise revision checks; a formula sheet; and 21 year-wise PYQs with answers.
Study Approach
Visualise. Read atoms, planes, defects and test geometry before using a formula.
Calculate. Choose the model, convert units and state its assumptions.
Interpret. Distinguish stiffness, strength, ductility, toughness and hardness.
Key checks: true-stress conversion needs its valid deformation range; the Schmid factor cannot exceed 0.5 in uniaxial loading; hardness-strength estimates are material-specific.
1. Materials engineering: structure, processing and properties
Materials engineering explains how atomic bonding, crystal arrangement, microstructure and processing determine the useful behaviour of a component. A shaft must resist twist; a spring must store recoverable energy; a cutting insert must resist indentation and wear. The same material family can behave differently after a change in grain size, deformation history or defect population.
Four linked questions: What is the structure? How was it produced? Which mechanisms operate under load? Which measured property represents the required service? A tensile strength is not a universal design strength, and a hardness number is not a complete description of toughness or ductility. Always connect a property to its test conditions and intended use.
Unit focus: start with unit cells and imperfections, then connect dislocation movement to yielding and strengthening. Finally interpret tensile, compression, torsion and hardness tests. Phase equilibria and detailed heat-treatment schedules belong to later units; here the emphasis is the structure-property and measurement foundations.
2. Atomic bonding and the origin of elastic response
Atoms in a solid adopt an equilibrium separation because attractive and repulsive interactions balance. A small change in separation produces a restoring force. The slope of the interatomic force-separation relation near equilibrium contributes to elastic stiffness. This atomic picture explains why elastic deformation is mostly recoverable when bonds return towards their original spacing.
Metals: metallic bonding allows delocalised electrons and generally non-directional bonding. Many metals can accommodate substantial plastic deformation by dislocation movement. Ceramics: ionic and covalent bonding often impose stronger restrictions on charge arrangement and available deformation mechanisms. Many engineering ceramics are stiff and hard but relatively intolerant of tensile flaws at ordinary temperature.
These are useful trends, not absolute rules. Crystal structure, temperature, composition, porosity, defects and loading rate also matter. Do not equate stronger bonding with higher ductility, or assume that strengthening a metal must significantly increase its Young’s modulus. Stiffness and resistance to plastic flow describe different mechanisms.
3. Crystal, lattice, basis and unit cell
A crystal has long-range periodic atomic order. A lattice is a repeating geometrical array of equivalent points; a basis is the atom or group of atoms attached to each point. Crystal structure = lattice + basis. A lattice point is therefore not automatically one individual atom, especially in compounds.
A unit cell is a repeatable volume that generates the lattice by translation. Its edges are a, b and c, and the angles between them are α, β and γ. A primitive cell contains one lattice point in total; a conventional cell may contain several and is often chosen to display symmetry more clearly. Cubic cells have a = b = c and all inter-edge angles equal to 90°.
Reading a cell: an atom drawn on a boundary is shared with neighbouring cells. Counting full spheres in a sketch gives the wrong cell population unless sharing is considered. Unit-cell pictures also exaggerate spacing or use small spheres so that positions remain visible; they need not represent atoms as isolated solid balls with empty space between them.
4. Counting atoms, coordination and packing factor
A corner atom of a three-dimensional cell contributes 1/8 to that cell; a face-centred atom contributes 1/2; an atom on an edge contributes 1/4; an atom fully inside contributes one. Add these fractions before using the number of atoms in a density or packing calculation.
Coordination number is the number of nearest neighbours of an atom in the ideal structure. Atomic packing factor is the volume occupied by ideal hard-sphere atoms assigned to the cell divided by the cell volume. For a cubic cell, APF = n(4πr³/3)/a³. It is a geometrical model, not a direct measurement of all electronic space occupied in a real solid.
A high packing factor does not by itself prove high strength or high hardness. Close-packed FCC metals can be ductile because of favourable slip systems. For density, use the correct cell population, atomic mass and edge length in consistent units; a cell dimension in nanometres cannot be inserted unchanged into a centimetre-based expression.
| Location | Fraction counted per cell |
|---|---|
| Corner | 1/8 |
| Face centre | 1/2 |
| Edge centre | 1/4 |
| Cell interior | 1 |
5. Simple cubic structure: a useful reference
The simple cubic cell has atoms at eight corners and no additional face or body atom. Its effective population is 8×1/8 = 1 atom per conventional cell. Nearest neighbours lie along the cube edges, so contact gives a = 2r. Each atom has six nearest neighbours.
APF = (4πr³/3)/(2r)³ = π/6 = 0.524 approximately. The structure is less densely packed than BCC, FCC and ideal HCP. Although it is not the common structure of most engineering metals, it is an important reference for understanding sharing, nearest-neighbour directions and packing calculations.
Do not mix contact directions: the edge-contact relation a = 2r applies to simple cubic. BCC contact occurs along the body diagonal and FCC contact along a face diagonal. Using the simple cubic relation for every cubic structure is a common numerical error.
6. Body-centred cubic structure
A BCC conventional cell contains eight corner atoms and one body-centre atom. The effective population is 8×1/8 + 1 = 2. The nearest neighbours of a body-centre atom are the eight corner atoms, giving coordination number 8.
Atoms contact along the body diagonal: √3a = 4r, so a = 4r/√3. Substitution into the hard-sphere expression gives APF = π√3/8 = 0.680 approximately. α-iron at ordinary temperature, chromium and tungsten are familiar BCC examples. The stable structure can change with temperature; an element should not be assigned one structure for all conditions.
BCC has no truly close-packed plane. Its slip behaviour is more temperature-sensitive than a simple count of possible slip systems might suggest. Many geometrically possible slip systems do not imply that all are equally easy to activate. Composition, temperature and dislocation-core resistance influence plastic deformation.
7. Face-centred cubic structure
An FCC conventional cell contains eight corner atoms and six face-centre atoms. Its effective population is 8×1/8 + 6×1/2 = 4 atoms. Each atom has 12 nearest neighbours. Aluminium, copper, nickel and γ-iron in its stability range are common examples.
Contact lies along a face diagonal: √2a = 4r, giving a = 2√2r. The ideal hard-sphere packing factor is π/(3√2) = 0.740. The close-packed planes are {111}, and the close-packed directions within them are <110>. There are 12 distinct {111}<110> slip systems when equivalent senses are counted conventionally.
The availability of several easy slip systems helps many FCC metals deform plastically at ordinary temperature. However, FCC structure alone does not guarantee high toughness in every material state. Alloying, defects, grain structure and the service environment still influence behaviour.
8. Hexagonal close packing and stacking sequence
HCP consists of close-packed atomic layers with an ABAB stacking sequence. FCC can also be described using close-packed layers, but its sequence is ABCABC. The ideal nearest-neighbour coordination is 12 and ideal APF is 0.740 for both structures. Their different stacking symmetry affects possible deformation modes.
The conventional hexagonal prism contains six effective atoms: shared corner and basal-face atoms together with three atoms fully inside the prism. Its volume is (3√3/2)a²c. The primitive HCP cell has a two-atom basis; therefore a statement that “HCP has two atoms” or “six atoms” must name the chosen cell. For ideal hard-sphere HCP, c/a = √(8/3) = 1.633; actual metals may differ.
Magnesium, α-titanium and zinc are examples of HCP metals. Basal slip is important in many HCP metals, but non-basal slip and twinning can also contribute. Do not state that every HCP material has only three possible slip systems under every condition; temperature and c/a ratio affect which mechanisms are accessible.
9. Comparing metallic crystal structures
Use a comparison table to separate geometry from mechanical behaviour. Population and contact direction belong to the chosen conventional cell; coordination and packing describe the ideal structure. These values are useful for density, radius and packing numericals, but they are not direct rankings of component strength.
A polycrystalline engineering metal contains grains with different orientations. Each grain retains its local crystal structure while its axes differ from those of neighbouring grains. The measured bulk response depends on how these grains deform together, as well as on pores, second phases and processing history.
Memory aid: cubic population 1-2-4 for SC-BCC-FCC; coordination 6-8-12; packing approximately 0.52-0.68-0.74. For HCP remember “same ideal close packing as FCC, different stacking sequence”. Never transfer a cubic cell-volume formula to the hexagonal prism.
| Structure | n | CN | Contact | APF |
|---|---|---|---|---|
| SC | 1 | 6 | a = 2r | 0.524 |
| BCC | 2 | 8 | √3a = 4r | 0.680 |
| FCC | 4 | 12 | √2a = 4r | 0.740 |
| HCP (conv.) | 6 | 12 | a = 2r; ideal c/a = 1.633 | 0.740 |
10. Crystal directions, planes and slip notation
A direction [uvw] identifies an oriented line using components referred to the crystallographic axes. A plane (hkl) is obtained from the reciprocals of its intercepts in lattice units, reduced to suitable integers. Square brackets refer to a direction; round brackets refer to a plane; angle brackets and braces describe families of equivalent directions and planes.
For a cubic cell, a plane cutting the x-axis at a and parallel to y and z is (100). A plane cutting x and y at a and parallel to z is (110). A plane cutting all three axes at a is (111). A parallel axis has an infinite intercept and hence a reciprocal index of zero. Choose an equivalent plane if the original passes through the origin.
In cubic crystals, [hkl] is normal to (hkl); this simple relation is not universal for non-cubic systems. A slip direction must lie in its slip plane. The notation {111}<110> does not mean every <110> direction lies in every {111} plane; select only compatible plane-direction combinations.
11. Theoretical density of a crystalline material
For an elemental crystalline solid, theoretical density ρ = nM/(NA Vc), where n is atoms per chosen cell, M is molar atomic mass, NA is Avogadro’s constant and Vc is cell volume. For cubic cells Vc = a³. Use n = 2 for conventional BCC and n = 4 for conventional FCC.
The calculation describes an ideal crystal of the stated composition and lattice parameter. Measured bulk density can be lower because of porosity or other microstructural features. A compound requires the total mass of its formula units in the selected cell; using one constituent’s atomic mass alone is incorrect.
Unit route: with M in g/mol and a in cm, density emerges in g/cm³. One nanometre is 10⁻⁷ cm, so a cubic nanometre is 10⁻²¹ cm³. Alternatively, use kg/mol and metres throughout for kg/m³. State the input temperature if lattice expansion matters; avoid mixing a room-temperature cell size with an unrelated high-temperature structure.
12. Ceramics: bonding, structure and response
Ceramics are inorganic nonmetallic materials that commonly involve ionic, covalent or mixed bonding. Engineering examples include alumina, silicon carbide and silicon nitride. Glasses are also important ceramic-family materials but lack long-range crystalline order; “ceramic” does not automatically mean “crystalline”.
Ionic crystal arrangements must preserve overall electrical neutrality. The relative ion sizes, charges and bonding determine feasible coordination. In a rock-salt-type structure, each ion has six nearest neighbours of opposite charge. Such compounds require a lattice-plus-basis description rather than treating both ions as identical spheres in a metallic cell.
Many engineering ceramics show high stiffness, hardness, wear resistance and useful temperature capability. Their tensile strength can be highly sensitive to flaws because substantial dislocation-mediated plastic relaxation is often difficult at room temperature. Compression suppresses opening of many cracks, so compressive and tensile behaviour can differ strongly. Porosity and processing quality remain critical; do not confuse hardness with immunity to brittle fracture.
13. Why real solids contain imperfections
An ideal crystal is a geometrical reference. Real solids contain vacancies, solute atoms, dislocations, boundaries, pores and inclusions. Imperfections are not always harmful: controlled solutes and obstacles can strengthen a metal, while uncontrolled cracks or large voids can reduce reliability.
Classify defects by dimensional extent. Point defects are localised around atomic sites. Line defects are dislocations. Interfacial defects extend over surfaces, such as grain boundaries or stacking faults. Volume defects occupy a three-dimensional region, such as a pore, inclusion or crack population. A crack has a surface geometry, but engineering classifications often group cracks among bulk or volume imperfections because of their component-scale extent.
The important question is how a defect interacts with diffusion, dislocation movement, stress concentration or crack growth. A label alone does not explain the property change. Specify defect type, distribution, scale and loading condition before deciding whether it strengthens, weakens or otherwise changes the material.
14. Vacancies, interstitials and substitutional atoms
A vacancy is an unoccupied normal lattice site. A self-interstitial is an extra host atom at an interstitial position; it usually causes substantial local distortion. An impurity atom may substitute for a host atom or occupy an interstitial site. Carbon in iron is an important interstitial-solute example.
Point defects distort surrounding bonds and can interact with moving dislocations. They also provide or modify diffusion pathways. A solute’s effect depends on size misfit, chemical interaction and concentration, not merely on being “foreign”. The atom distribution and the surrounding structure must be considered.
Do not call a substitutional solute a vacancy, or assume that an interstitial must be another atom of the same species. A self-interstitial and an interstitial impurity are different cases. The diagram uses simplified atomic positions; real local displacements are distributed over several neighbouring atoms.
15. Thermal vacancies and defect concentration
Vacancies can be present at thermal equilibrium because their formation increases configurational entropy while costing energy. A simple dilute model gives Nv/N = exp[-Qv/(kB T)], where Qv is vacancy formation energy per vacancy, kB is Boltzmann’s constant and T is absolute temperature. The model omits additional entropy factors unless explicitly included.
Use compatible energy units. If Qv is in eV, use kB = 8.617×10⁻⁵ eV/K. If energy is per mole, use the gas constant in a matching molar expression. Temperature in degrees Celsius must be converted to kelvin before substitution.
The exponential dependence means vacancy fraction usually rises rapidly with temperature. A quenched solid may retain a nonequilibrium defect population, so the equilibrium formula does not automatically describe every processed sample at its current temperature. Also distinguish the fraction Nv/N from the absolute number Nv; the latter requires a defined number of atomic sites.
16. Point defects in ionic solids
A Schottky defect consists of charge-balanced vacancies in an ionic crystal. For a simple AB compound with equal-magnitude ionic charges, the familiar schematic removes one cation and one anion. In other stoichiometries the vacancy ratio must preserve charge and composition appropriately; it is not universally one of each ion.
A Frenkel defect is a vacancy-interstitial pair formed when an ion leaves its regular site and occupies an interstitial position. The familiar case involves a small cation, but the defining feature is the paired displacement, not the use of a particular element. No atom has to leave the complete crystal for this rearrangement.
Schottky disorder generally reduces mass per crystal volume, while an idealised Frenkel rearrangement does not remove an ion from the specimen. Real density changes can also involve lattice relaxation. Draw charges and missing sites clearly: an unlabeled empty circle is not enough to distinguish a vacancy from an interstitial location.
17. Edge dislocations and the extra half-plane
An edge dislocation is a line defect associated with the termination of an extra half-plane of atoms inside a crystal. The dislocation line follows the edge of that terminating plane. The surrounding lattice is distorted, with a characteristic compressive region on one side and tensile region on the other in the simple elastic picture.
The Burgers vector b describes the magnitude and direction of the lattice displacement associated with the defect. For a pure edge dislocation, b is perpendicular to the dislocation line. A Burgers circuit constructed using the same step sequence as in a perfect reference lattice fails to close; the closure convention defines the vector direction.
Under a suitable resolved shear stress the dislocation can glide, allowing slip to proceed by local bond rearrangement rather than simultaneous translation of a whole plane. The extra half-plane picture is a useful schematic, not an assertion that a detached physical sheet has been inserted into an otherwise unstrained solid.
18. Screw and mixed dislocations
A screw dislocation produces a shear displacement that makes lattice planes form a helical ramp around the dislocation line. For a pure screw dislocation, the Burgers vector is parallel to the line. Its displacement character differs from the extra-half-plane picture of a pure edge dislocation.
Most real dislocation lines are curved and have mixed character: different segments may be closer to edge or screw orientation while sharing the relevant Burgers vector. The direction of b and the local line tangent determine the character. A single line need not remain purely edge throughout its length.
Dislocation movement depends on lattice resistance, obstacles and temperature. Screw segments may change between compatible glide planes through cross-slip, while climb of an edge component involves diffusion and is not the same as ordinary conservative glide. Unit I requires the basic distinction; do not describe all dislocation motion as an atom-free sliding of two rigid blocks.
19. Interfacial and volume defects
A grain boundary separates crystals of different orientation. A low-angle boundary can be represented as an arrangement of dislocations in a simple model; a high-angle boundary has a more complex atomic structure. A twin boundary separates mirror-related orientations, while a stacking fault interrupts the normal close-packed layer sequence.
Free surfaces are also interfaces because atoms lack neighbours present in the interior. Pores, inclusions and cracks introduce larger-scale discontinuities. Pores can reduce the load-bearing area; hard inclusions may impede motion locally but also initiate damage if poorly bonded or unfavourably shaped.
Do not assign one universal effect to every grain boundary. Boundaries can impede slip and strengthen many metals at ordinary temperature, but can also provide rapid diffusion paths or participate in high-temperature deformation. Likewise, refining grains is not a universal solution for every service condition. State the mechanism and temperature range.
20. Slip: how a crystal deforms plastically
Slip is permanent shear displacement on a crystallographic plane in a crystallographic direction. It is commonly carried by the movement of dislocations. Successive dislocation passages leave a net offset and produce measurable plastic strain even though only local bonds are rearranged at a given instant.
A slip system combines one slip plane with one allowed slip direction lying in that plane. Closely packed planes and short translation directions often offer favourable slip paths. Slip bands visible at a specimen surface are collective traces of deformation, not individual atomic dislocations viewed directly with the naked eye.
Elastic strain stretches bonds reversibly; plastic slip changes relative atomic registry and leaves a permanent shape change. A test may include both at the same time. On unloading after plastic deformation, the elastic part recovers while the slip-related strain remains. This distinction explains why unloading does not normally return a yielded specimen to its original length.
21. Slip systems in FCC, BCC and HCP metals
FCC slip commonly occurs on {111}<110>, giving 12 conventional systems. Several appropriately oriented systems can operate in a polycrystal. BCC slip uses <111> directions on families such as {110}, {112} and {123}; the common geometrical counts are 12, 12 and 24 respectively, but actual activity depends strongly on conditions.
HCP basal slip commonly uses the basal plane and an a-type close-packed direction. Basal systems alone cannot accommodate every general shape change in a polycrystal. Prismatic or pyramidal slip and twinning may contribute when stress and temperature make them accessible. A three-index cubic notation should not be applied carelessly to hexagonal directions.
Interpretation: structure and orientation influence how easily plasticity begins, but slip-system count is not a standalone measure of ductility. BCC metals can become difficult to deform at low temperature despite many possible systems. HCP alloys may show substantial formability when additional mechanisms are active.
| Crystal | Typical slip description | Important qualification |
|---|---|---|
| FCC | {111}<110>; 12 systems | Several easy systems often available |
| BCC | <111> on {110}, {112}, {123} | No close-packed plane; temperature-sensitive |
| HCP | Basal a-type often important | Non-basal slip and twinning can contribute |
22. Resolved shear stress and Schmid’s law
An applied uniaxial stress does not act entirely as shear on a selected slip system. Let φ be the angle between the loading axis and the slip-plane normal, and λ the angle between the loading axis and the slip direction. Resolved shear stress is τR = σ cosφ cosλ. The product m = cosφ cosλ is the Schmid factor.
The slip-plane area is larger than the cross-section normal to the force by the factor 1/cosφ, while the force component along slip is F cosλ. Combining the projected area and force gives the two cosine factors. Confusing the plane angle with its normal angle introduces an error.
The slip direction is perpendicular to the plane normal, so φ and λ are geometrically constrained. The maximum absolute Schmid factor under uniaxial loading is 0.5, reached for a suitable 45°-45° orientation. Arbitrarily selecting φ = λ = 0° is impossible for a valid plane-direction pair and does not produce m = 1 physically.
23. Critical resolved shear stress and orientation
The critical resolved shear stress, CRSS, is the resolved shear stress required to initiate the relevant slip under the stated conditions. In a simple single-crystal Schmid-law model, yielding begins when |σm| reaches τc. The tensile stress needed for that slip system is σy = τc/|m|, provided m is nonzero.
A favourably oriented crystal has a larger |m| and can begin slip at a smaller applied tensile stress for the same CRSS. If m = 0, the chosen system receives no resolved shear from that loading direction; another system may still be active. Compare all candidate systems rather than choose one arbitrarily.
CRSS depends on material state, temperature, solute content, obstacles and loading conditions. A polycrystal has compatibility constraints and multiple orientations, so the single-crystal formula is not by itself a complete bulk yield model. Do not insert the macroscopic proof stress as CRSS without a justified relationship.
24. Strengthening: obstructing dislocation movement
Many strengthening methods increase the stress required for dislocation movement. Solid-solution strengthening uses solute interactions; strain hardening increases dislocation interactions; grain refinement increases barriers to slip transfer; dispersed particles and precipitates provide additional obstacles. The mechanisms can act together.
Strengthening usually changes yield resistance more strongly than elastic modulus because it changes the difficulty of plastic rearrangement rather than the basic stiffness of interatomic bonds. Increased strength can be accompanied by reduced ductility, changed workability or altered toughness. The engineering choice requires a balance rather than simply maximising one number.
An obstacle diagram is a mechanism sketch, not a measured micrograph. Real strengthening depends on obstacle size, spacing, coherency, distribution and temperature. Extremely small grains or high-temperature service can involve additional mechanisms outside the simple introductory models.
25. Grain-size strengthening and Hall-Petch relation
For many polycrystalline metals over an appropriate grain-size range, σy = σ0 + ky d^(-1/2), where d is a representative grain size. Grain boundaries can inhibit slip transfer, so reducing grain size raises the stress needed for continued deformation in the simple picture.
Units matter: if d is in metres, ky must carry a compatible square-root metre factor with the chosen stress unit. Using a millimetre grain size with a metre-based coefficient changes the result by a large factor. A graph against d^(-1/2), rather than against d directly, is linear under the model.
The relation is empirical and range-dependent. It is not an exact atomic law for all grain sizes and temperatures. A useful calculation states σ0, ky, grain-size units and the assumed material condition. Grain refinement may also change toughness and processing behaviour, but a strength calculation alone does not quantify those changes.
26. Solid solutions, particles and strain hardening
Substitutional or interstitial solutes distort the lattice and can interact with dislocations. This makes glide more difficult in a suitable solid solution. Particle or precipitation strengthening adds obstacles that a dislocation may cut through or bypass depending on particle character and spacing; a larger particle is not automatically a more effective strengthening particle.
Cold working introduces plastic deformation below a temperature at which recovery and recrystallisation rapidly remove its effects on the chosen time scale. Increasing dislocation density promotes interactions and increases resistance to further slip. Yield strength and hardness often rise, while remaining ductility can fall.
Percentage cold work based on area is CW = (A0-Af)/A0 ×100. It describes an area reduction, not directly the true strain or the percentage increase in strength. Detailed recovery and heat-treatment pathways are treated later; here remember the distinction between storing deformation structure and changing the elastic modulus.
27. Mechanical testing: obtaining a valid property
A test converts measured force, displacement, geometry, torque or indentation into a property using a defined method. Reliable results require representative specimens, calibrated instruments, correct alignment and suitable data reduction. Report material condition, specimen dimensions, temperature and loading rate where they affect interpretation.
Separate an instrument reading from a material property. A force of 20 kN is not tensile strength until divided by the appropriate cross-sectional area. Crosshead travel includes machine and grip compliance and is not automatically the specimen gauge extension used to calculate strain or modulus.
Inspection after the test is important. Grip slippage, off-axis loading, fracture outside the gauge section, an inadequately prepared surface or a visibly asymmetric indentation may invalidate part of the result. A smooth plotted curve does not prove the setup was correct. Examine the complete measurement chain before reporting too many decimal places.
28. Tensile test: apparatus and specimen preparation
A tensile test applies increasing axial tension to a specimen held between grips. A load cell measures force. An extensometer or suitable strain-measurement system measures extension over a defined gauge length. The reduced gauge section encourages the deformation and fracture region to develop away from the gripping ends.
Measure original gauge length L0 and original area A0 before loading. For a circular specimen A0 = πd_0²/4; for a rectangular specimen A0 = width×thickness. Align the specimen axis with the load axis, choose appropriate grips and verify the strain measurement range. A strain gauge or extensometer must not be treated as a force sensor.
During the test record paired force-extension data, observe yielding and necking, and obtain the maximum force. After fracture, bring the pieces together to measure final gauge length according to the adopted method, and measure the minimum neck area if reduction in area is required. Avoid extrapolating an elastic extensometer beyond its permitted range.
29. Engineering stress and engineering strain
Engineering normal stress is σe = F/A0 and engineering strain is e = (L-L0)/L0 = ΔL/L0. Both use the original specimen dimensions. With force in newtons and area in mm², stress is N/mm², numerically equal to MPa. Strain is dimensionless; 0.002 strain equals 0.2%, not 2%.
The slope of the initial linear stress-strain relation gives Young’s modulus if the strain measurement is reliable and the material is in the appropriate linear range. A force-extension slope has units of stiffness, N/mm; convert using E = (L0/A0)(ΔF/ΔL). The same material can have different component stiffness when area or length changes.
The engineering curve is useful for comparing standardised tests, but its denominator remains A0 even after the gauge section changes. A drop after maximum engineering stress is therefore not by itself evidence that the local material flow stress has fallen. Necking and the distinction between original and instantaneous area become essential.
30. Reading a ductile engineering stress-strain curve
The initial linear segment describes approximately proportional elastic response. The proportional limit, elastic limit and specified proof stress are related but are not identical definitions. Some steels show an upper and lower yield point with a plateau; many other materials show a smooth transition without a distinct yield point.
After yielding, plastic deformation and strain hardening can raise the applied force. The ultimate tensile strength is the maximum engineering stress, Fmax/A0. At the onset of diffuse necking in a conventional ductile tensile test, deformation becomes less uniform. Fracture occurs later at a localised region, often after the engineering load has fallen.
Label the horizontal axis as engineering strain and the vertical axis as engineering stress. A schematic curve is not universal: brittle materials can fracture with little plastic strain, and the amount of yielding or strain hardening depends on material condition. Do not draw a long mild-steel yield plateau for every metal.
31. Yield strength and the 0.2% proof-stress construction
Yielding marks the onset of significant permanent deformation under the chosen criterion. A distinct yield stress can sometimes be read directly from the curve. When the transition is smooth, a specified proof stress is obtained by an offset construction rather than by guessing where the curve appears to bend.
For 0.2% proof stress, draw a line parallel to the initial elastic line but starting at engineering strain 0.002. Its intersection with the measured stress-strain curve defines the proof stress. The offset is a strain, not 0.2% of the vertical stress scale or 0.2 mm of arbitrary extension.
Use an appropriately resolved strain measurement; a coarse plot may not determine proof stress accurately. Do not claim that the offset point is a perfectly sharp microscopic first motion of a dislocation. It is a reproducible engineering criterion associated with the specified nonproportional strain.
32. True stress and logarithmic strain
True stress uses the instantaneous area: σt = F/A. True or logarithmic axial strain for uniform extension is εt = ∫dL/L = ln(L/L0). Engineering strain instead divides the entire extension by L0. For small strain, ln(1+e) is close to e; at large strain the difference becomes important.
For uniform uniaxial plastic extension with approximately constant volume, AL = A0L0. Therefore A0/A = L/L0 = 1+e, giving σt = σe(1+e) and εt = ln(1+e). The logarithmic relation follows directly from uniform length change; the stress conversion additionally uses the volume assumption.
These conversions must not be applied blindly to the whole gauge length after necking. Deformation is then nonuniform and the neck stress state is not simply uniaxial. A local area measurement and, for some flow-stress interpretations, a triaxiality correction are needed. Label plotted post-necking extensions as conceptual unless the actual local data and correction are available.
33. Uniform deformation, necking and strain measures
During uniform tensile extension, the gauge section deforms approximately throughout its length. Necking localises deformation into a smaller region. The ordinary global gauge extension no longer uniquely determines the minimum local area, so a uniform-volume conversion based on total gauge length becomes unreliable.
For a useful idealisation of uniaxial uniform plastic flow with constant volume, local logarithmic plastic strain can be related to area by ln(A0/A). This is a geometrical interpretation, not permission to ignore the multiaxial stress near a developed neck. Do not use σt = F/A as if it were automatically the equivalent flow stress in every necked geometry.
The maximum engineering stress and the fracture engineering stress are different quantities. Likewise, the final elongation measured after fracture contains the localised contribution and is not simply the uniform elongation at UTS. State which strain measure and stage of the test are being discussed before comparing values.
34. Ductility: elongation and reduction in area
Ductility describes the capacity for plastic deformation before fracture under specified conditions. Two common tensile measures are percentage elongation = (Lf-L0)/L0 ×100 and percentage reduction in area = (A0-Af)/A0 ×100. Here Lf is the reconstructed final gauge length and Af is the minimum final area.
Elongation depends on the chosen gauge length and specimen geometry because localised neck deformation contributes differently to short and long gauge lengths. Reduction in area describes local contraction at the neck. The two percentages need not be equal and should not be substituted for one another.
A high-strength material can still have useful ductility, and a soft material need not have high toughness. Compare tests made under compatible conditions and distinguish tensile ductility from formability under another stress state. When a fracture occurs outside the intended gauge section, follow the adopted test method before accepting the elongation result.
35. Young’s modulus and component stiffness
Young’s modulus E is the slope dσ/dε in the appropriate linear uniaxial elastic range. For a uniform prismatic bar, axial extension is ΔL = FL/(AE), provided small strain, axial loading and the relevant material assumptions apply. Axial component stiffness is k = AE/L.
E is a material parameter for a specified direction and condition; k is a property of the component and setup. Doubling area doubles k without changing E. A longer gauge section gives more extension under the same force and area, again without changing the material modulus.
The initial toe of a force-extension record can include seating, straightening and grip effects. Use the valid elastic segment and suitable strain instrumentation rather than treat the first two raw machine points as a precise modulus measurement. For anisotropic crystals, modulus depends on orientation; a single isotropic E represents an approximation to the bulk response of a suitable material.
36. Compression test: measurement and interpretation
A compression test loads a specimen axially between platens. A short cylindrical specimen is commonly used to reduce the risk of column buckling. Measure its original area and length, apply aligned loading and obtain force-shortening data. Compressive stress and strain may be reported as positive magnitudes or negative signed values; define the convention.
For engineering magnitudes, σc = F/A0 and ec = (L0-L)/L0. The signed axial strain is negative under the usual tension-positive convention. Friction at the platens restrains lateral expansion near the ends and can produce barreling. The result then differs from ideal homogeneous uniaxial compression.
Ductile metals may flatten substantially without the tensile-style fracture used to define elongation. Brittle materials can have much greater compressive than tensile strength because compression tends to close cracks instead of opening them. Slender-specimen buckling is a structural instability and must not be mistaken for the intrinsic compressive strength of the material.
37. Torsion test of a circular specimen
A torsion test applies torque T and measures angular twist θ over gauge length L. A solid circular elastic shaft has polar second moment J = πd⁴/32; a hollow shaft has J = π(D⁴-d⁴)/32. Under small elastic twist, τ(r) = Tr/J and θ = TL/(GJ).
The maximum shear stress occurs at the outer radius R, giving τmax = TR/J. The surface engineering shear strain is γmax = Rθ/L with θ in radians. The slope of torque against angle, TL-related through geometry, can be used to determine the shear modulus G. Degrees must be converted to radians before substitution.
These elastic formulas do not remain a complete stress distribution after plastic yielding spreads through the cross-section. The specimen must be circular and appropriately uniform for the simple expressions. Grips, alignment, backlash and angle measurement affect the result. State whether a quoted torque is the first-yield torque, maximum torque or another selected criterion.
38. Poisson’s ratio, shear and bulk moduli
Under uniaxial elastic tension, many materials contract laterally. Poisson’s ratio is ν = -εtransverse/εaxial. For ordinary positive ν, tensile axial strain is positive and transverse strain negative, producing a positive ratio. Negative-Poisson-ratio materials exist; do not define ν as necessarily positive by taking absolute values silently.
Shear modulus G relates shear stress to engineering shear strain: τ = Gγ in the linear range. Bulk modulus K relates hydrostatic pressure to volumetric strain with a consistent sign convention. For isotropic linear elasticity, E = 2G(1+ν) and E = 3K(1-2ν). Only two of E, G, K and ν are independent under this assumption.
The relations do not hold unchanged for a general anisotropic single crystal. Also, engineering shear strain γ is twice the corresponding off-diagonal tensor strain component in small-strain notation. State the convention before writing a constitutive matrix; otherwise a factor-of-two error can appear even when the numerical shear stress is correct.
39. Generalised Hooke’s law for isotropic elasticity
For a homogeneous isotropic linear elastic material at small strain, εx = [σx-ν(σy+σz)]/E, with cyclic expressions for εy and εz. The shear relations are γxy = τxy/G, γyz = τyz/G and γzx = τzx/G. Tensile normal stress is positive in the convention used here.
These expressions combine direct extension with Poisson coupling from the other normal stresses. For example, a tensile σy contributes a contraction -νσy/E in the x direction even if σx is zero. Treating each normal strain as σ/E independently ignores this coupling.
The law is a constitutive relation, not an equilibrium equation. It must be used with suitable loading, compatibility and boundary conditions. It excludes substantial plasticity, large-strain geometry and arbitrary crystal anisotropy. If temperature changes are included, add the appropriate thermal strains rather than assume that every measured strain is mechanically produced.
40. Plane stress, plane strain and hydrostatic loading
Plane stress idealises a thin region with negligible out-of-plane stresses: σz = τ_xz = τyz = 0. The out-of-plane strain is generally not zero; for isotropic linear elasticity εz = -ν(σx+σy)/E. Thin sheets loaded in their plane are a common application away from local constraints.
Plane strain instead imposes εz = γ_xz = γyz = 0 in the chosen direction. A nonzero σz is generally needed to enforce that restraint. Do not set both σz and εz to zero automatically in a multiaxial problem.
For equal hydrostatic compressive normal stresses -p, εv = εx+εy+εz = -3p(1-2ν)/E = -p/K. This separates volume change from shape distortion in the small-strain isotropic model. General yielding under multiaxial stress requires an appropriate yield criterion; the uniaxial tensile yield value is not an independent allowable for each component without further reasoning.
41. Resilience and recoverable strain energy
Resilience is the ability to store and release elastic strain energy. The modulus of resilience Ur is the elastic energy per unit volume up to the chosen elastic or yield limit. For uniaxial linear elasticity, Ur = ∫σdε = σy²/(2E) when σy is the applicable upper elastic-boundary approximation.
The area under a stress-strain curve has units of energy per volume: Pa = J/m³. If stress and E are both in MPa, the computed energy density in MPa is numerically MJ/m³. Total energy additionally requires multiplication by the volume over which the relevant stress-strain state applies.
A high modulus alone does not guarantee high resilience. With the same yield strength, increasing E reduces σy²/(2E); with higher yield strength, resilience can increase strongly. Spring materials require an appropriate combination of elastic limit, geometry, fatigue performance and environment, not just one large textbook number.
42. Toughness, strength and stiffness are different
Tensile toughness is the energy absorbed per unit volume up to fracture, represented by the area under the complete tensile stress-strain curve on the stated measurement basis. It combines stress level and deformation capacity. A very strong but brittle material may absorb less total tensile energy than a moderately strong ductile material.
Toughness is not the same as the elastic energy measure resilience. It is also not the same as fracture toughness, which characterises crack resistance using a particular crack configuration and validity conditions. An impact energy from a notched test has another measurement basis and cannot simply be read as area under an ordinary unnotched tensile curve.
Comparison: stiffness describes elastic resistance to deformation; strength describes resistance to a specified yielding or failure criterion; ductility describes plastic deformation before fracture; hardness describes resistance in a specified indentation procedure. Use the property that answers the design question and avoid treating all four as synonyms.
43. Elastic recovery and residual plastic strain
When a specimen is unloaded from a plastic deformation state, the recoverable elastic strain decreases while permanent plastic strain remains. In a simple linear-unloading approximation, εtotal = εe + εp and εe = σ/E at the unloading point. The residual strain after complete unloading is εp.
On a stress-strain diagram, draw the unloading line with approximately the elastic slope E. Its intercept on the strain axis represents residual strain. The recovered strain is the horizontal difference between the loaded point and that intercept. This construction is approximate if unloading is nonlinear, damage changes stiffness or time-dependent effects are important.
Elastic recovery is not the same as complete recovery of the original microstructure. A cold-worked specimen can retain dislocations and hardening after the elastic portion returns. A metal forming operation may therefore show springback even while substantial permanent shape change remains.
44. Hardness: what an indentation actually measures
Indentation hardness measures resistance to local deformation under a defined indenter, force and procedure. A hardness number depends on the measurement method and scale. Brinell, Vickers and Rockwell values are not interchangeable raw numbers, even when obtained from the same material.
Choose a representative, sufficiently thick specimen with a suitable surface. Avoid placing indentations too close to an edge or another indentation, and consider roughness, curvature, coatings and microstructural variation. A surface-hardened case and the softer core can produce different results depending on penetration and load.
Hardness tests are useful for quality control, comparing material condition and detecting local variation. They do not directly measure tensile ductility or toughness. Any conversion to tensile strength needs a material-specific empirical basis and an appropriate validity range; it is not a substitute for a required tensile test.
45. Brinell hardness: ball indentation
Brinell testing uses a hard ball, commonly tungsten carbide in modern practice, pressed into the surface under a specified test force. Measure the residual indentation diameter after unloading, often along two perpendicular directions and average them. The ball diameter is D and the indentation diameter is d.
Using force F in newtons and D, d in mm, HBW = 0.102×2F/[πD(D-√(D²-d²))]. Using force expressed in kgf, omit the 0.102 conversion factor. The denominator represents the curved spherical indentation area, not simply the projected circular area πd²/4.
The relatively large impression can average over a coarse microstructure but may be unsuitable for a thin layer or small finished component. Report the method and test conditions, not a bare number. A measured d must be less than D for this geometry; an impossible diameter or an asymmetric impression calls for investigation rather than a forced calculation.
46. Vickers hardness: diamond-pyramid indentation
Vickers testing uses a square-based diamond pyramid with an angle of 136° between opposite faces. Measure the two diagonals d_1 and d_2 of the residual impression and use their mean d. The indentation is represented as a diamond-shaped square in a plan view, with both diagonals clearly marked.
With F in newtons and d in mm, HV = 0.1891F/d². With force in kgf, HV = 1.8544F/d². Do not mix these constants or insert a diagonal measured in micrometres without converting it to millimetres. The squared denominator makes small measurement errors important.
A wide range of test forces makes Vickers useful for bulk and smaller-scale hardness assessment when the specimen and surface are suitable. Low-force results can be sensitive to preparation, focus, diagonal recognition and indentation-size effects. The measured impression is not a direct image of individual crystal slip systems.
47. Rockwell hardness: residual depth and scale
Rockwell testing measures a permanent indentation-depth increment rather than optically measuring the impression width. A preliminary force establishes a reference; an additional force produces the total test force; after the additional force is removed, depth is read while the preliminary force remains.
A conventional Rockwell value has the form HR = N-h/S, where h is the measured residual depth increment and N and S depend on the scale family. For a conventional diamond scale such as HRC, N = 100 and S = 0.002 mm. Do not use this expression unchanged for superficial Rockwell scales or every ball scale.
The chosen scale defines the indenter and force combination. HRC uses a diamond cone with a rounded tip; common ball scales use the specified ball size. Always report the scale letters with the number. “60 Rockwell” is incomplete because 60 HRC and 60 on another scale do not describe the same test condition.
48. Comparing hardness methods and test quality
Brinell and Vickers are optical indentation-size methods; Rockwell uses residual depth. The preferred method depends on material condition, microstructure, specimen size, thickness, surface and the region being measured. A larger indentation averages a larger volume but can damage a small component more severely.
Before accepting a result, check the support, surface finish, load selection, calibration and impression geometry. A thin specimen can deform against the support; a curved surface can bias the reading; an indentation near an edge or another impression can interact with its affected zone. Use the adopted procedure for limits rather than one invented spacing rule for every scale.
Repeat measurements at suitable locations and report both representative value and variation where appropriate. A large spread may reflect real microstructural heterogeneity or a measurement problem. Do not erase inconvenient results without investigating their cause.
| Method | Indenter / measured quantity | Useful feature |
|---|---|---|
| Brinell | Ball / residual diameter | Larger sampled region |
| Vickers | Diamond pyramid / mean diagonal | Wide force range; small regions possible |
| Rockwell | Specified cone or ball / residual depth | Direct scale reading; efficient routine testing |
49. Hardness-strength relations and their limits
For selected steels and suitable hardness ranges, an approximate empirical relation is tensile strength in MPa ≈ 3.45×HB. The factor relates a conventional Brinell number to a tensile-strength estimate for an appropriate material class. It is not an exact physical identity and should not be applied automatically to aluminium, ceramics or every steel condition.
Hardness relates to resistance to local plastic flow, while a tensile test measures an evolving uniaxial response and eventual instability or fracture. Strain hardening, microstructure and indentation conditions affect the relationship. Case-hardened surfaces, coatings or strongly heterogeneous materials can make a surface hardness especially unrepresentative of bulk tensile strength.
Use a supplied conversion or approved material-specific relation when an examination question requests an estimate. Label the result approximate and state the validity assumption. Never convert a hardness reading directly into fracture toughness, fatigue strength or guaranteed allowable design stress without an additional justified model.
50. Integrated structure-property-test selection
Choose the measurement by the required information. Tensile testing gives elastic slope, a yield or proof criterion, UTS and tensile ductility. Compression testing addresses crushing or compressive deformation without confusing buckling with material failure. Torsion gives torque-twist response and, in its elastic range, shear modulus and shear-stress distribution for a suitable specimen.
Hardness is useful for rapid local condition comparison, but it samples an indentation response. Crystal and defect analysis explains why the response changes. For example, cold working can increase dislocation interactions and hardness while reducing remaining ductility, even though the elastic modulus changes relatively little.
A complete exam answer should contain a definition, mechanism or apparatus, labelled sketch where relevant, governing relation with units, and limitations. For a numerical, write the known data, choose a compatible model, substitute consistently and interpret the result. Distinguish an idealised teaching calculation from an experimentally verified property of a real component.
SOLVED PROBLEMS: STRUCTURE, TESTING AND PROPERTIES
All numerical input data are teaching examples. Use the stated crystal model, test geometry, loading range and units. They are not certified properties, current standard limits or guaranteed design values.
Worked problem 1.1: Theoretical BCC iron density
Use atomic mass 55.85 g/mol and BCC lattice parameter 0.2866 nm. Find ideal density using NA = 6.022×10²³ mol⁻¹.
- 1. Cell atoms n = 2; a = 2.866×10⁻⁸ cm.
- 2. Vc = (2.866×10⁻⁸)³ = 2.35412×10⁻²³ cm³.
- 3. Cell mass = 2×55.85/(6.022×10²³) = 1.85487×10⁻²² g.
- 4. ρ = cell mass/cell volume ≈ 7.879 g/cm³.
Answer. ρ ≈ 7.88 g/cm³.
Check. This ideal crystal value excludes specimen porosity; 1 g/cm³ = 1000 kg/m³.
Worked problem 1.2: Hexagonal cell and ideal height
For an ideal HCP crystal with a = 0.320 nm, find c and the conventional hexagonal cell volume.
- 1. Use ideal c/a = √(8/3) = 1.632993.
- 2. c = 0.320×1.632993 = 0.522558 nm.
- 3. V = (3√3/2)a²c = 0.13902 nm³.
Answer. c ≈ 0.52256 nm; V ≈ 0.13902 nm³.
Check. This is the six-atom conventional prism, not a cube or the two-atom primitive cell.
Worked problem 1.3: Miller indices from intercepts
A plane intercepts crystal axes at 2a, 3b and infinity along c. Determine its Miller indices.
- 1. Write intercepts in lattice units: 2, 3, ∞.
- 2. Take reciprocals: 1/2, 1/3, 0.
- 3. Multiply by 6 to remove fractions: 3, 2, 0.
Answer. The plane is (320).
Check. A parallel axis produces index zero, not an infinite index.
Worked problem 1.4: Thermal vacancy fraction
Assume Qv = 1.0 eV, T = 1000 K and kB = 8.617×10⁻⁵ eV/K. Estimate equilibrium vacancy fraction using the simple dilute model.
- 1. Nv/N = exp[-Qv/(kB T)].
- 2. Exponent = -1/(8.617×10⁻⁵×1000) = -11.60497.
- 3. Nv/N ≈ 9.1207×10⁻⁶.
Answer. About 9.12 vacancies per million lattice sites under the model.
Check. The number is a fraction, not 9.12%; temperature is already in kelvin.
Worked problem 1.5: Resolved shear stress
A single crystal is loaded at 100 MPa. For a compatible slip system, φ = 60° and λ = 30°. Find resolved shear stress.
- 1. m = cos60° cos30° = 0.433013.
- 2. τR = σm = 100×0.433013.
- 3. τR = 43.3013 MPa.
Answer. τR ≈ 43.30 MPa.
Check. φ refers to the slip-plane normal; these coplanar angles sum to 90° and are compatible.
Worked problem 1.6: Hall-Petch grain refinement
Use σ0 = 70 MPa and ky = 0.74 MPa·m^(1/2). Compare yield stresses for grain sizes 100 μm and 25 μm.
- 1. Convert d_1 = 1.00×10⁻⁴ m; d_2 = 2.50×10⁻⁵ m.
- 2. σ_1 = 70 + 0.74/√(1.00×10⁻⁴) = 144 MPa.
- 3. σ_2 = 70 + 0.74/√(2.50×10⁻⁵) = 218 MPa.
- 4. Increase = 74 MPa.
Answer. 144 MPa and 218 MPa; refinement increases the model strength by 74 MPa.
Check. The coefficient uses metres; inserting grain size as a bare micrometre number is wrong.
Worked problem 1.7: Engineering tensile stress and strain
A specimen has original diameter 10 mm and gauge length 50 mm. At a 20 kN load its measured gauge extension is 0.080 mm. Determine engineering stress and strain.
- 1. A0 = π×10²/4 = 78.5398 mm².
- 2. σe = 20,000/78.5398 = 254.648 MPa.
- 3. e = 0.080/50 = 0.0016 = 0.16%.
Answer. σe ≈ 254.65 MPa; e = 0.0016.
Check. The paired reading alone does not prove that the point is elastic; do not infer E without a valid elastic-range assumption.
Worked problem 1.8: Convert engineering to true measures
Before necking, a uniformly deforming tensile specimen has engineering stress 300 MPa and engineering strain 0.20. Assume constant plastic volume. Find true stress and true strain.
- 1. σt = σe(1+e) = 300×1.20 = 360 MPa.
- 2. εt = ln(1+e) = ln1.20 = 0.182322.
- 3. Use the uniform-region and volume assumptions explicitly.
Answer. True stress 360 MPa; logarithmic strain 0.18232.
Check. Do not use the same conversion for a developed neck from global gauge strain alone.
Worked problem 1.9: Compression stress and shortening
A 20 mm diameter, 40 mm long cylinder is compressed by 0.20 mm under 100 kN. Use engineering magnitudes.
- 1. A0 = π×20²/4 = 314.159 mm².
- 2. σc = 100,000/314.159 = 318.310 MPa.
- 3. ec = 0.20/40 = 0.005 = 0.5%.
Answer. Compressive stress magnitude 318.31 MPa; strain magnitude 0.005.
Check. Under the tension-positive sign convention, the corresponding axial stress and strain are negative.
Worked problem 1.10: Torque, shear stress and angle
A solid circular elastic shaft has d = 20 mm, L = 500 mm, G = 80 GPa and torque 100 N·m. Find maximum shear stress and twist.
- 1. Use T = 100,000 N·mm and G = 80,000 N/mm².
- 2. J = π×20⁴/32 = 15,707.963 mm⁴.
- 3. τmax = TR/J = 100,000×10/15,707.963 = 63.662 MPa.
- 4. θ = TL/(GJ) = 0.0397887 rad = 2.27973°.
Answer. τmax ≈ 63.66 MPa; twist ≈ 0.03979 rad = 2.28°.
Check. The section is circular and assumed elastic. The radian value is the one used in the constitutive equation.
Worked problem 1.11: Generalised Hooke law under three normal stresses
Use E = 200 GPa, ν = 0.30 and normal stresses σx = 100, σy = 50, σz = -20 MPa. Find the three normal strains and volumetric strain.
- 1. E = 200,000 MPa.
- 2. εx = [100-0.3(50-20)]/200,000 = 0.000455.
- 3. εy = [50-0.3(100-20)]/200,000 = 0.000130.
- 4. εz = [-20-0.3(100+50)]/200,000 = -0.000325.
- 5. εv = εx+εy+εz = 0.000260.
Answer. εx = 455 με; εy = 130 με; εz = -325 με; εv = 260 με.
Check. Check εv = (1-2ν)(σx+σy+σz)/E = 0.4×130/200,000.
Worked problem 1.12: Modulus of resilience
A linearly elastic material reaches the chosen yield limit at 400 MPa with E = 200 GPa. Estimate its modulus of resilience.
- 1. Use consistent MPa units: E = 200,000 MPa.
- 2. Ur = σy²/(2E) = 400²/(2×200,000).
- 3. Ur = 0.40 MPa = 0.40 MJ/m³.
Answer. 0.40 MJ/m³ of elastic energy density.
Check. This is energy per volume, not total joules or tensile toughness to fracture.
Worked problem 1.13: Toughness from discrete test data
Approximate energy density up to fracture using engineering points (strain, MPa): (0,0), (0.002,400), (0.10,500), (0.20,300). Use trapezoids.
- 1. Area 1 = (0+400)/2×0.002 = 0.4 MPa.
- 2. Area 2 = (400+500)/2×(0.10-0.002) = 44.1 MPa.
- 3. Area 3 = (500+300)/2×(0.20-0.10) = 40.0 MPa.
- 4. Total = 84.5 MPa = 84.5 MJ/m³.
Answer. Approximate tensile energy density = 84.5 MJ/m³.
Check. This is a numerical area estimate on the supplied engineering curve, not a measured fracture-toughness parameter.
Worked problem 1.14: Brinell hardness with kgf input
A 10 mm ball produces a 4 mm mean indentation under 3000 kgf. Calculate the conventional Brinell number.
- 1. Use HB = 2F/[πD(D-√(D²-d²))] because F is in kgf.
- 2. √(D²-d²) = √84 = 9.16515 mm.
- 3. HB = 6000/[π×10×(10-9.16515)] = 228.77 approximately.
Answer. Approximately 229 HBW on the stated load and ball basis.
Check. Do not multiply by 0.102 again when the force is already expressed in kgf.
Worked problem 1.15: Vickers hardness and diagonal averaging
A Vickers test uses 30 kgf. Indentation diagonals are 0.40 and 0.42 mm. Find HV.
- 1. Mean diagonal d = (0.40+0.42)/2 = 0.410 mm.
- 2. HV = 1.8544F/d² for kgf input.
- 3. HV = 1.8544×30/(0.410)² = 330.946.
Answer. Approximately 331 HV, with the test force stated.
Check. Average the measured diagonals first; do not average two independently rounded hardness numbers.
Worked problem 1.16: Rockwell depth calculation
For a conventional HRC teaching calculation, residual depth increment h = 0.080 mm. Use HRC = 100-h/0.002. Find the reading.
- 1. h/0.002 = 0.080/0.002 = 40.
- 2. HRC = 100-40 = 60.
- 3. Include the scale letters in the reported result.
Answer. 60 HRC.
Check. This scale relation does not apply unchanged to superficial Rockwell or every ball scale.
QUICK REVISION: QUESTIONS WITH ANSWERS
Does a large APF guarantee a strong metal?
No. Packing factor describes ideal geometrical filling. Yield strength also depends on dislocation mobility, obstacles, grain size, temperature and composition. An FCC metal can be readily ductile despite its high packing factor because it has favourable slip systems.
How do Schottky and Frenkel defects differ?
Schottky disorder involves charge-balanced vacancies. Frenkel disorder moves an ion from a normal site into an interstitial position, creating a vacancy-interstitial pair. The familiar one-cation plus one-anion Schottky sketch assumes a compatible AB compound, not every possible ionic stoichiometry.
What is the maximum uniaxial Schmid factor?
The maximum absolute value is 0.5 for a suitable orientation. The slip direction and plane normal are perpendicular, which constrains the two angles with the loading axis. Taking both angles as zero, or choosing incompatible small angles, cannot create a physical factor of one.
When can engineering stress be converted by σt = σe(1+e)?
Use it for uniform tensile deformation with the stated approximately constant-volume assumption. After necking, global gauge strain no longer determines the local neck area. The neck also has a multiaxial stress state, so further local measurements and interpretation are required.
Why is buckling not a compressive material strength?
A slender specimen can become unstable because of geometry, end conditions and stiffness before its material reaches the intended compressive failure condition. A short compression specimen reduces this problem. A column collapse cannot automatically be reported as intrinsic crushing strength.
Which torsion formulas are restricted to the elastic range?
The linear distribution τ = Tr/J and the twist relation θ = TL/(GJ) describe a suitable circular shaft under the stated elastic assumptions. Once plastic yielding spreads, the elastic stress distribution does not remain valid throughout the cross-section.
Can plane stress have nonzero thickness strain?
Yes. With σz = 0, isotropic elasticity gives εz = -ν(σx+σy)/E. Setting thickness strain to zero introduces an additional constraint associated with a plane-strain model and generally changes the required out-of-plane stress.
Can hardness replace a tensile test?
Only a qualified empirical estimate is possible for suitable material conditions and correlation ranges. Surface cases, coatings and heterogeneous structures can be unrepresentative of bulk response. Hardness does not directly give tensile elongation, fracture toughness or a universal allowable design stress.
FORMULAS AND DECISION QUICK REFERENCE
| Quantity / concept | Relation and limitation |
|---|---|
| Cubic atom counts | SC 1; BCC 2; FCC 4 |
| Cubic contact | SC a=2r; BCC √3a=4r; FCC √2a=4r |
| APF | n(4πr³/3)/Vc; ideal hard spheres |
| HCP conventional cell | 6 atoms; Vc=(3√3/2)a²c; ideal c/a=1.633 |
| Theoretical density | ρ=nM/(NA Vc); match mass and length units |
| Thermal vacancies | Nv/N=exp[-Qv/(kB T)]; T in kelvin |
| Schmid law | τR=σ cosφ cosλ; maximum |m|=0.5 |
| First slip | σ=τc/|m| for selected system |
| Hall-Petch | σy=σ0+ky/√d; stated empirical range |
| Cold work | 100(A0-Af)/A0 |
| Engineering tension | σe=F/A0; e=ΔL/L0 |
| True measures | σt=F/A; εt=ln(L/L0) for uniform extension |
| Uniform conversion | σt=σe(1+e), with constant-volume assumption |
| Young modulus | E=Δσ/Δε in the valid linear range |
| Bar stiffness | k=AE/L; component geometry matters |
| Poisson ratio | ν=-εtransverse/εaxial |
| Isotropic elastic constants | G=E/[2(1+ν)]; K=E/[3(1-2ν)] |
| Generalised normal strain | εx=[σx-ν(σy+σz)]/E; cyclic forms |
| Engineering shear | γxy=τxy/G |
| Volume strain | εv=(1-2ν)(σx+σy+σz)/E |
| Solid circular torsion | J=πd⁴/32; τmax=TR/J; θ=TL/(GJ) |
| Ductility | Elongation=100ΔL/L0; RA=100(A0-Af)/A0 |
| Resilience | Ur=σy²/(2E) for linear response |
| Toughness | Area under stated tensile curve to fracture |
| Residual strain | εp=εtotal-σ/E for linear unloading |
| Brinell, F in N | HBW=0.102×2F/[πD(D-√(D²-d²))] |
| Vickers | HV=0.1891FN/d² = 1.8544Fkgf/d² |
| Conventional HRC example | HRC=100-h/0.002; h in mm |
| Approximate steel relation | UTS(MPa)≈3.45 HB; only suitable correlation range |
| Energy density conversion | 1 MPa=1 MJ/m³; multiply by m³ for joules |
PYQs WITH ANSWERS – UNIT I
Questions from the five supplied papers, grouped by examination year, with original numbers, marks and answers. Labelled sketches accompany the questions that require them.
| Marks | Theory target | What to include |
|---|---|---|
| 2 | 40-60 words | Direct definition or requested points; a formula or example where useful. |
| 7 | 150-200 words | A short introduction, organised explanation or comparison, and a relevant sketch. |
| 10 | 250-300 words | A complete structured explanation, key distinctions and a relevant example, table or diagram. |
Writing guide: These are practical targets, not prescribed AKTU word limits. Follow the exact question. For numericals, show given data, assumptions, formula, substitution, units and the final result; do not add prose just to meet a word count.
EXAMINATION 2021-22 | KME303
Q1 (2021-22)
Original Q1(a) | Section A | 2 marks
Define unit cell in a crystal structure.
Answer
A unit cell is a repeating geometrical volume that, when translated through the lattice, reproduces the crystal arrangement. It is described by three edge lengths and three interaxial angles, together with the atomic basis. A conventional cell is chosen for convenience and symmetry; it need not be the smallest possible primitive cell.
Q2 (2021-22)
Original Q1(b) | Section A | 2 marks
Differentiate between ductility and malleability.
Answer
Ductility is the ability to undergo plastic deformation in tension, commonly assessed by percentage elongation or reduction in area. Malleability is the ability to undergo plastic deformation under compression, as in rolling or hammering into sheets. Both describe plastic deformability, but the loading mode and practical forming operation differ.
Q3 (2021-22)
Original Q1(d) | Section A | 2 marks
Draw the plane having miller indices (011) and (001).
Answer
For a cubic cell of edge a, the (011) plane has intercepts ∞, a, a: it is parallel to x and satisfies y + z = a. The (001) plane has intercepts ∞, ∞, a: it is parallel to x and y and satisfies z = a. The labelled sketches show these intercepts.
Q4 (2021-22)
Original Q2(a) | Section B | 10 marks
Classify the defect in crystal and explain point defect in detail with neat sketch.
Answer
1. Classification. Crystal imperfections are grouped by dimensionality: point defects such as vacancies and solute atoms; line defects such as dislocations; interfacial defects such as grain and twin boundaries; and volume defects such as pores, inclusions and cracks.
2. Vacancy. A regular lattice site is unoccupied. Vacancies enable important diffusion processes, and their equilibrium concentration increases with temperature. A vacancy is a missing atom, not a small pore made of many missing sites.
3. Self-interstitial. An extra solvent atom occupies a normally unoccupied interstitial position and distorts nearby atomic positions. An interstitial solute, such as carbon in iron, occupies a site between regular solvent positions.
4. Substitutional solute. A foreign atom replaces a solvent atom at a normal site. Differences in size and bonding produce local strain and can impede dislocation movement.
5. Ionic crystals. Schottky defects involve charge-balanced vacancy combinations; a Frenkel defect involves an ion displaced to an interstitial position, leaving a vacancy. Electrical neutrality must be maintained.
6. Engineering significance. Point defects affect diffusion, electrical behaviour and mechanical response. Draw and label a perfect site, vacancy, substitutional atom and interstitial separately; do not use one unidentified circle for every defect.
7. For a dilute equilibrium vacancy model, the vacancy fraction is approximately exp[-Qv/(kT)] when Qv is the vacancy-formation energy per atom. This relation describes a supplied ideal model; it is not a pore-volume formula.
Q5 (2021-22)
Original Q3(a) | Section C | 10 marks
Discuss the stress strain curve for steel and explain why steel is having two yield points. Also establish relation between the true stress and engineering stress.
Answer
1. Axes and initial region. Plot engineering stress F/A0 against engineering strain ΔL/L0. The initial linear elastic slope is Young’s modulus. Beyond the elastic range, permanent strain remains on unloading.
2. Upper and lower yield. Some low-carbon steels show an upper yield point followed by a lower yield level and a yield plateau. Interstitial solutes can pin dislocations; their release and subsequent plastic propagation help explain discontinuous yielding and Lüders deformation. Not every steel shows two distinct yield points.
3. Strain hardening and necking. After yielding, increasing plastic deformation raises the flow stress. Engineering stress reaches the ultimate tensile strength and then falls as necking localises deformation. Final fracture occurs after further local reduction of area.
4. Stress conversion. Engineering stress uses original area A0; true stress uses instantaneous area A. Before necking, under the usual approximately constant-volume plastic assumption, AL = A0 L0. With engineering strain e, A = A0/(1 + e), giving σtrue = σeng(1 + e).
5. Strain conversion and limits. True strain is ∫dL/L = ln(L/L0) = ln(1 + e) for uniform extension. After necking, the gauge-average engineering strain cannot supply the local neck area; measure the current local area for true stress. The descending engineering branch does not mean the local material has necessarily softened.
6. For elastic unloading, the approximate strain recovered is σ/E when the stress and modulus use a consistent small-strain convention. The remaining intercept is plastic strain. This is distinct from the total extension reached before unloading.
Q6 (2021-22)
Original Q3(b) | Section C | 10 marks
A component having length of 1m was loaded beyond elastic limit. At a point when its length increased by 3mm. It was experiencing stress of 250MPa. If the young’s modulus of the material is 200GPa. What will be the final dimension of the component after unloading.
Answer
1. Given and assumption. Original length L0 = 1 m = 1000 mm; total extension at peak loading = 3 mm; stress = 250 MPa; E = 200 GPa = 200000 MPa. Take the quoted stress as engineering stress and assume linear elastic unloading without reverse yielding.
2. Total engineering strain. etotal = 3/1000 = 0.003.
3. Recoverable elastic strain. eelastic = σ/E = 250/200000 = 0.00125.
4. Permanent plastic strain. eplastic = 0.003 – 0.00125 = 0.00175.
5. Recovered extension. ΔLelastic = 1000 × 0.00125 = 1.25 mm. The loaded length is 1003 mm.
6. Final dimension. Lfinal = 1003 – 1.25 = 1001.75 mm = 1.00175 m. Equivalently, the permanent extension is 1000 × 0.00175 = 1.75 mm.
7. Check. The final length lies between the original and maximum loaded lengths. Returning to 1000 mm would wrongly assume all strain was elastic; retaining 1003 mm would ignore elastic recovery. The result uses the small-strain convention normally intended by the supplied data.
EXAMINATION 2022-23 | KME-303
Q7 (2022-23)
Original Q1(a) | Section A | 2 marks
Define Unit Cell.
Answer
A unit cell is a repeating geometrical volume that, when translated through the lattice, reproduces the crystal arrangement. It is described by three edge lengths and three interaxial angles, together with the atomic basis. A conventional cell is chosen for convenience and symmetry; it need not be the smallest possible primitive cell.
Q8 (2022-23)
Original Q1(b) | Section A | 2 marks
Define Malleability.
Answer
Malleability is the capacity of a material to undergo substantial plastic deformation under compression without cracking. It is important in hammering, rolling and forming sheets. Gold and many copper or aluminium products are familiar examples. It differs from ductility, which commonly refers to plastic deformation in tension, such as wire drawing.
Q9 (2022-23)
Original Q2(a) | Section B | 10 marks
Explain the Crystal Structure (System) in detail.
Answer
1. Crystal system versus metallic structure. A crystal system specifies cell-edge and angle relationships. There are seven crystal systems and fourteen Bravais lattices. A lattice with its atomic basis defines the complete crystal structure.
2. Cubic. a = b = c and α = β = γ = 90°. Simple cubic, BCC and FCC are cubic lattice types. In a metallic hard-sphere description, BCC has two effective atoms per conventional cell and FCC four.
3. Other edge relationships. Tetragonal has a = b ≠ c with right angles; orthorhombic has three unequal edges with right angles. Monoclinic has three unequal edges, conventionally α = γ = 90° and β ≠ 90°.
4. Nonorthogonal systems. Triclinic has no imposed equalities of edges or angles. Hexagonal uses a = b ≠ c, α = β = 90° and γ = 120°. Trigonal can use a rhombohedral cell with equal edges and equal angles not equal to 90°.
5. Sketch and examples. Label a, b, c and the angles on a unit cell. Compare BCC alpha iron, FCC copper and HCP magnesium as common metallic structures. HCP is hexagonal with a basis, not an additional fifteenth Bravais lattice. Cell symmetry and atom arrangement should be stated separately.
Q10 (2022-23)
Original Q3(a) | Section C | 10 marks
Discuss the Line Imperfections with the help of neat sketches.
Answer
1. Definition. A dislocation is a line imperfection associated with a lattice-displacement mismatch. Its direction and Burgers vector describe its geometry. Dislocation motion allows plastic slip at stresses much lower than those required to shear a perfect crystal uniformly.
2. Edge dislocation. An extra half-plane of atoms terminates within the crystal. The dislocation line follows the termination, and the Burgers vector is perpendicular to that line. The surrounding lattice has a characteristic distortion field.
3. Screw dislocation. Relative shear gives planes a helical arrangement around the dislocation line. The Burgers vector is parallel to the line. A screw segment can access different suitable slip planes by cross-slip under appropriate conditions.
4. Mixed dislocation. A curved dislocation generally contains both edge and screw character. The Burgers vector remains associated with the same dislocation, while the local line direction changes.
5. Importance. Slip produces permanent deformation as dislocations move. Solutes, precipitates, grain boundaries and other dislocations impede that movement, providing strengthening. High dislocation density can increase strength while reducing ductility.
6. Sketch requirements. Mark the extra half-plane, line direction and perpendicular Burgers vector for edge character. For screw character, label the line and parallel Burgers vector. Distinguish a line defect from a two-dimensional grain boundary.
Q11 (2022-23)
Original Q3(b) | Section C | 10 marks
Explain the Load-Deformation diagram for a brittle material.
Answer
1. Axes. A load-deformation diagram plots applied force vertically and extension or displacement horizontally. For a uniform axial specimen in linear elasticity, F = (EA/L0)ΔL, so the initial structural stiffness is EA/L0.
2. Typical brittle response. A brittle material commonly exhibits a mostly elastic rising branch and fractures with little macroscopic plastic deformation. There is no long yielding plateau or extensive tensile necking in the ideal sketch. The exact shape depends on material and loading conditions.
3. Energy. The area under the force-displacement curve is work, with units of energy. In a linear approximation up to fracture, it is Ff ΔLf/2. The area under a stress-strain curve instead represents energy per unit volume.
4. Interpretation. A steep line indicates high specimen stiffness, not automatically high toughness. Stiffness also depends on dimensions. Brittle specimens can have substantial compressive strength while being much less tolerant of tensile flaws.
5. Comparison. A ductile tensile specimen usually has a larger plastic extension and can absorb more energy before fracture under comparable conditions. Temperature, notch constraint and strain rate can change the observed response, so a material family should not be assigned an immutable brittle label.
EXAMINATION 2023-24 | BME303
Q12 (2023-24)
Original Q1(a) | Section A | 2 marks
Define unit cell in crystal structure.
Answer
A unit cell is a repeating geometrical volume that, when translated through the lattice, reproduces the crystal arrangement. It is described by three edge lengths and three interaxial angles, together with the atomic basis. A conventional cell is chosen for convenience and symmetry; it need not be the smallest possible primitive cell.
Q13 (2023-24)
Original Q2(b) | Section B | 7 marks
Classify the defect in crystal and explain point defect in detail with neat sketch.
Answer
1. Classification. Crystal imperfections are grouped by dimensionality: point defects such as vacancies and solute atoms; line defects such as dislocations; interfacial defects such as grain and twin boundaries; and volume defects such as pores, inclusions and cracks.
2. Vacancy. A regular lattice site is unoccupied. Vacancies enable important diffusion processes, and their equilibrium concentration increases with temperature. A vacancy is a missing atom, not a small pore made of many missing sites.
3. Self-interstitial. An extra solvent atom occupies a normally unoccupied interstitial position and distorts nearby atomic positions. An interstitial solute, such as carbon in iron, occupies a site between regular solvent positions.
4. Substitutional solute. A foreign atom replaces a solvent atom at a normal site. Differences in size and bonding produce local strain and can impede dislocation movement.
5. Ionic crystals. Schottky defects involve charge-balanced vacancy combinations; a Frenkel defect involves an ion displaced to an interstitial position, leaving a vacancy. Electrical neutrality must be maintained.
6. Engineering significance. Point defects affect diffusion, electrical behaviour and mechanical response. Draw and label a perfect site, vacancy, substitutional atom and interstitial separately; do not use one unidentified circle for every defect.
EXAMINATION 2024-25 | BME303
Q14 (2024-25)
Original Q2(a) | Section B | 7 marks
With the help of neat sketch explain different types of crystal structure.
Answer
1. Meaning. A crystal structure combines a repeating lattice with an atomic basis. FCC, BCC and HCP are common metallic arrangements; the table gives the ideal hard-sphere comparison.
2. BCC. Atoms occupy the cube corners and body centre. The effective count is 8 × 1/8 + 1 = 2. Contact is along the body diagonal, so √3 a = 4r. The coordination number is eight and APF is approximately 0.68.
3. FCC. Atoms occupy corners and face centres. The count is 8 × 1/8 + 6 × 1/2 = 4. Contact along a face diagonal gives √2 a = 4r. Coordination number is twelve and APF is approximately 0.74.
4. HCP. Close-packed planes follow an ABAB stacking sequence. Coordination number is twelve and ideal APF is approximately 0.74. The ideal c/a ratio is about 1.633; actual metals can differ.
5. Examples and interpretation. Ferritic iron, tungsten and chromium are BCC; aluminium, copper and nickel are FCC; magnesium, zinc and alpha titanium are HCP. Packing factor alone does not determine strength or ductility, because bonding, slip, temperature and microstructure also matter.
| Structure | CN | Ideal APF |
|---|---|---|
| BCC | 8 | 0.68 |
| FCC | 12 | 0.74 |
| HCP | 12 | 0.74 |
Q15 (2024-25)
Original Q3(a) | Section C | 7 marks
Draw a neat sketch of BCC crystal structure and calculate its atomic packing factor and also find out the effective number of atoms.
Answer
1. Arrangement. A conventional BCC cell contains atoms at eight corners and one atom at the body centre. Each corner contributes one eighth to the cell; the centre atom belongs completely to it.
2. Effective atom count. n = 8 × 1/8 + 1 = 2 atoms per conventional cell. The coordination number is eight.
3. Contact geometry. In the ideal hard-sphere model, atoms touch along the body diagonal. Its length is √3 a and it contains four radii, so √3 a = 4r and a = 4r/√3.
4. Occupied volume. The two spheres contribute Vatoms = 2(4πr³/3) = 8πr³/3.
5. Cell volume and APF. Vcell = a³ = (4r/√3)³. Hence APF = Vatoms/Vcell = π√3/8 = 0.680, approximately 68%.
6. Check and examples. BCC is less densely packed than ideal FCC or HCP, whose APF is about 0.74. Alpha iron and tungsten are examples. Label edge a, radius r and the body diagonal on the sketch; using the face diagonal would incorrectly apply FCC geometry.
Q16 (2024-25)
Original Q3(b) | Section C | 7 marks
NaCl structure has FCC structure. The density of NaCl is 2.18 g/cm³. Calculate the distance between two adjacent atoms.
Answer
1. Interpret the structure. Rock-salt NaCl has two interpenetrating FCC sublattices. Its conventional cubic cell contains four NaCl formula units, or four Na⁺ and four Cl⁻ ions. The nearest neighbours are unlike ions, separated by a/2 along a cube edge.
2. Supply missing constants. Use MNa = 22.99 g/mol, MCl = 35.45 g/mol and NA = 6.022 × 10^23 mol⁻¹. Therefore the NaCl molar mass is 58.44 g/mol. These are declared values because the paper supplies only density.
3. Cell mass. mcell = 4M/NA = 4 × 58.44/(6.022 × 10^23) = 3.882 × 10^(-22) g.
4. Cell volume. a³ = mcell/ρ = 3.882 × 10^(-22)/2.18 = 1.781 × 10^(-22) cm³.
5. Cell edge and adjacent-ion distance. a ≈ 5.626 × 10^(-8) cm = 0.5626 nm. Thus nearest-neighbour Na-Cl spacing = a/2 ≈ 0.2813 nm.
6. Clarify the wording. The paper says adjacent atoms; for this ionic crystal the physically intended nearest pair is Na⁺-Cl⁻. Nearest same-sublattice neighbours are instead a/√2 ≈ 0.3978 nm. Do not use a monatomic-FCC count of four atoms for the entire NaCl cell.
EXAMINATION 2025-26 | BME303
Q17 (2025-26)
Original Q1(a) | Section A | 2 marks
Define Hooke’s law in its generalized form? What is the difference between engineering stress and true stress?
Answer
Generalised linear elasticity is σij = Cijkl εkl for the stated elastic range. For an isotropic material, εx = [σx – ν(σy + σz)]/E and γxy = τxy/G. Engineering stress is load/original area; true stress is load/current area. Plastic deformation is not described by Hooke’s law.
Q18 (2025-26)
Original Q1(b) | Section A | 2 marks
What is a dislocation? Differentiate between line and interfacial defects.
Answer
A dislocation is a line defect associated with a displacement mismatch in the crystal; edge, screw and mixed dislocations are examples. Interfacial defects extend over surfaces rather than lines, such as grain boundaries, twin boundaries and phase interfaces. Dislocation motion enables plastic slip, whereas interfaces can hinder or interact with that motion.
Q19 (2025-26)
Original Q2(a) | Section B | 7 marks
Define toughness and resilience? How is toughness measured from a stress-strain curve?
Answer
1. Resilience. Resilience is the ability to absorb recoverable elastic energy. The modulus of resilience is the area under the elastic stress-strain curve up to the defined elastic/yield limit. For a linear uniaxial model, Ur = σy²/(2E).
2. Toughness. Tensile toughness is the energy absorbed per unit original volume up to fracture in the specified tensile test. It includes elastic and plastic contributions: Ut = ∫σeng de over the engineering curve to fracture.
3. How to measure. Record load and extension, convert them to engineering stress and strain, plot the curve and integrate the area to fracture. Numerical integration may use a sum of trapezoidal areas when discrete points are supplied.
4. Units and comparison. Stress in Pa times dimensionless strain gives J/m³; MPa corresponds to MJ/m³ for the integrated area. A material combining strength and extensive plastic deformation can have a large area, while a strong but brittle specimen may have a much smaller area.
5. Important distinction. Tensile toughness is not the same quantity as fracture toughness KIC or impact-test energy. Each is determined under a different test geometry and loading condition. Draw the elastic area separately from the full area to fracture.
Q20 (2025-26)
Original Q3(a) | Section C | 7 marks
Define Young’s modulus. Differentiate between engineering stress-strain and true stress-strain curves. Derive the relation between stress-strain.
Answer
1. Young’s modulus. E is the ratio of normal stress to corresponding normal elastic strain in uniaxial linear elasticity. It is the initial elastic slope, not the ultimate strength or hardness.
2. Definitions. Engineering stress S = F/A0 and engineering strain e = (L – L0)/L0 use original dimensions. True stress σ = F/A and true strain ε = ∫dL/L use the instantaneous geometry and incremental extension.
3. Derive true strain. Integrating from L0 to L gives ε = ln(L/L0) = ln(1 + e). For very small strain, ln(1 + e) is approximately e.
4. Derive true stress. Before necking, use the stated approximately constant-volume plastic model: AL = A0 L0. Therefore A0/A = L/L0 = 1 + e, and σ = (F/A0)(A0/A) = S(1 + e).
5. Curve interpretation. The engineering tensile curve can fall after its maximum because necking reduces the load-bearing section. A true curve based on measured local area may continue rising. The conversion using gauge engineering strain is valid only while the assumed uniform deformation and volume relation hold; do not apply it indiscriminately after necking.
Q21 (2025-26)
Original Q3(b) | Section C | 7 marks
Describe the common metallic crystal structures (FCC, BCC, HCP). Compare their packing efficiency, coordination number, and examples of metals exhibiting these structures.
Answer
1. Meaning. A crystal structure combines a repeating lattice with an atomic basis. FCC, BCC and HCP are common metallic arrangements; the table gives the ideal hard-sphere comparison.
2. BCC. Atoms occupy the cube corners and body centre. The effective count is 8 × 1/8 + 1 = 2. Contact is along the body diagonal, so √3 a = 4r. The coordination number is eight and APF is approximately 0.68.
3. FCC. Atoms occupy corners and face centres. The count is 8 × 1/8 + 6 × 1/2 = 4. Contact along a face diagonal gives √2 a = 4r. Coordination number is twelve and APF is approximately 0.74.
4. HCP. Close-packed planes follow an ABAB stacking sequence. Coordination number is twelve and ideal APF is approximately 0.74. The ideal c/a ratio is about 1.633; actual metals can differ.
5. Examples and interpretation. Ferritic iron, tungsten and chromium are BCC; aluminium, copper and nickel are FCC; magnesium, zinc and alpha titanium are HCP. Packing factor alone does not determine strength or ductility, because bonding, slip, temperature and microstructure also matter.
| Structure | CN | Ideal APF |
|---|---|---|
| BCC | 8 | 0.68 |
| FCC | 12 | 0.74 |
| HCP | 12 | 0.74 |